Method for preparing monatomic mercury catalyst by using waste mercury catalyst as raw material and product thereof
Through catalytic gasification extraction and adsorption of defective carbon support, the complexity of waste mercury catalyst recycling technology and environmental pollution were solved, and high-performance single-atom mercury catalyst and chlorinated defective carbon support were prepared, which improved mercury and carbon resources. Utilization efficiency.
Patent Information
- Application Number
- CN202410915270.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-07-09
AI Technical Summary
The existing waste mercury catalyst recycling technology is complex, the environmental pollution is large, the mechanical strength of the recovered carbon carrier is poor, the pore structure and surface structure are damaged, and the recovery rate of mercury chloride is low.
The mercury chloride is extracted by catalytic gasification, and the mercury chloride gasification aid is used to heat up in an inert gas stream for catalytic gasification. The mercury chloride is absorbed by defective carbon support to capture it, and a single-atom mercury catalyst is prepared and obtained by pulverizing and bonding. High-performance chlorinated defective carbon carrier.
The preparation of high-performance single-atom mercury catalyst and high-performance chlorinated defective carbon support is realized, which improves the recovery rate of mercury chloride and the application value of carbon materials, simplifies the process flow, and reduces environmental pollution.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of waste mercury catalyst recycling and mercury catalyst preparation, and in particular to a method for preparing a single-atom mercury catalyst using waste mercury catalyst as a raw material and a product thereof. Background Art
[0002] Mercury catalyst is an important industrial catalyst for producing vinyl chloride (acetylene-based vinyl chloride) from acetylene and hydrogen chloride. Mercury catalysts will be deactivated after a certain period of use and will be removed from the vinyl chloride production unit to become waste mercury catalysts. Waste mercury catalysts contain 2-3wt.% of mercuric chloride. Since mercuric chloride is highly toxic, arbitrary disposal of waste mercury catalysts will cause serious environmental pollution. Therefore, waste mercury catalysts are listed as hazardous waste disposal. At the same time, mercury, as an important heavy metal resource, plays an important role in catalysts, drugs, and devices for special scenarios. However, due to the increasing depletion of mercury resources stored in nature, how to recycle existing mercury resources is particularly important. Therefore, efficient recycling of waste mercury catalysts can not only prevent mercury waste from harming the natural environment, but also recycle mercury resources to achieve huge economic benefits.
[0003] At present, the technology for recycling waste mercury catalysts mainly focuses on how to extract mercury from waste mercury catalysts. The methods for recovering mercury mainly include liquid phase washing method, high temperature distillation method and dry distillation method. In the liquid phase washing method, competitive adsorbents such as NaCl and hydrochloric acid are added to desorb mercuric chloride from the surface of activated carbon into the solution, and then the mercuric chloride is reduced to elemental mercury for recovery with reducing agents such as formaldehyde. Although the recovery process is simple to operate, the recovery rate of mercuric chloride is relatively low, only about 60%. In the high temperature distillation method, NaOH, lime and other treatment agents are first added to convert the mercuric chloride on the surface of activated carbon into mercuric oxide, and then heated to 700-800℃ to decompose the mercuric oxide into mercury vapor, and then condensed to recover elemental mercury. In the process of high temperature distillation, inorganic salts such as lime are added to promote the volatilization of mercuric chloride. However, the addition of inorganic salts such as lime makes the ash impurities of the carbon carrier after mercury extraction as high as 50% or more. Even if acid washing and other treatments are performed, high-performance activated carbon cannot be obtained. The dry distillation method directly heat treats the waste mercury catalyst at 500-600°C in a nitrogen atmosphere to desorb the mercuric chloride on the activated carbon into the gas phase, and then condenses and recovers the mercuric chloride. The mercury chloride is used to prepare the mercury catalyst again by the impregnation method, which is a complicated process.
[0004] In summary, the current waste mercury catalyst recovery method first adds chemical reagents for treatment, then washes or high-temperature heat treatment to extract mercury elements, then prepares elemental mercury, and then prepares mercuric chloride. The entire recovery process is complex and environmentally polluting. In addition, the current treatment of waste mercury catalysts is mainly aimed at refining residual mercury. The recovered carbon carrier has poor mechanical strength due to crushing, collision and wear during the use of the catalyst, and soaking or heat treatment during the catalyst recovery process; and in order to improve the recovery rate of mercuric chloride, a large amount of chemical additives are added during the recovery process, which makes the ash content of the recovered activated carbon high and complex, the pore structure is poor, and the surface structure is severely damaged. Summary of the invention
[0005] In view of the above technical problems and the deficiencies in the art, the present invention provides a method for preparing a single-atom mercury catalyst using a waste mercury catalyst as a raw material, using catalytic gasification to extract mercuric chloride and prepare a single-atom mercury catalyst. The process is simple, and the waste catalyst treatment and the preparation of a new catalyst are integrated. While treating the waste mercury catalyst, a high-performance single-atom mercury catalyst and a chlorination defect carbon carrier are prepared. The recovered chlorination defect carbon carrier is an excellent carrier for the single-atom mercury catalyst to capture mercuric chloride, realizing the application of recycled carbon materials in this field, making full use of mercury resources and carbon resources, and making high-value use of waste mercury catalysts.
[0006] A method for preparing a single-atom mercury catalyst using waste mercury catalyst as a raw material, comprising:
[0007] The waste mercury catalyst is mixed with a mercuric chloride gasification aid, and then heated to 300-350° C. (preferably 300° C.) in an inert gas flow for catalytic gasification, and the mercuric chloride in the catalytic gasification tail gas is adsorbed and captured by a defective carbon carrier to obtain a single-atom mercury catalyst; the heating rate is 30-100° C. / min;
[0008] The mercuric chloride gasification aid includes at least one of potassium nitrate, sodium nitrate, barium nitrate, zinc nitrate and cerium nitrate.
[0009] In some embodiments, the spent mercury catalyst has a water content of less than 3 wt %.
[0010] The present invention promotes the volatilization of mercuric chloride by using a mercuric chloride gasification aid. In some embodiments, the mass ratio of the mercuric chloride gasification aid to the waste mercury catalyst is 1-5:10, preferably 2:10.
[0011] The defective carbon support may include a chlorinated defective carbon support.
[0012] In some embodiments, the defective carbon support used in the present invention includes a chlorinated defective carbon support prepared by recovering the waste mercury catalyst after catalytic gasification. The chlorinated defective carbon support not only has a high adsorption intensity and a large adsorption amount for mercuric chloride, but also the doping of heteroatom chlorine improves the exchange process of chlorine in HCl and HgCl2 in the acetylene hydrochlorination reaction, thereby improving the reaction rate and increasing the reaction activity of the catalyst.
[0013] Furthermore, the preparation method of the chlorinated defective carbon carrier may include: mixing the solid product of the catalytic gasification with an activator and a binder, grinding and crushing them, kneading them into a shape, drying them, and carbonizing them in an inert atmosphere to obtain the chlorinated defective carbon carrier.
[0014] In some embodiments, in the method for preparing the chlorinated defective carbon support, the activator may include at least one of melamine, dicyandiamide, urea, and cyanuric acid. The above activators can promote the cross-linking and preliminary carbonization of vinyl chloride in the carbon deposits of the waste mercury catalyst, and the mercuric chloride gasification aid remaining in the catalytic gasification process can become a defect inducer in the high-temperature carbonization process to form a chlorinated defective carbon support.
[0015] In some embodiments, in the method for preparing the chlorinated defective carbon support, the mass ratio of the activator to the waste mercury catalyst may be 1-5:10.
[0016] The present invention uses a binder to bond the ground waste mercury catalyst carbon carrier after mercury extraction to form a granular chlorinated defective carbon carrier. In some embodiments, in the preparation method of the chlorinated defective carbon carrier, the binder may include at least one of gelatinized starch, humate, and phenolic resin. The humate may be an ammonium salt or the like.
[0017] In some embodiments, in the method for preparing the chlorinated defective carbon support, the mass ratio of the binder to the waste mercury catalyst may be 1-5:10.
[0018] In some embodiments, in the method for preparing the chlorinated defective carbon support, the carbonization temperature can be 800-900° C., preferably 850° C., and the time can be 2-4 hours, preferably 3 hours.
[0019] In the method for preparing the chlorinated defective carbon carrier, the inert atmosphere refers to a gas atmosphere that does not participate in the reaction, such as a nitrogen atmosphere and / or a rare gas atmosphere such as argon.
[0020] In some embodiments, the mass ratio of the defective carbon support to the spent mercury catalyst may be 1:1-10, preferably 1:1.
[0021] In the present invention, the inert gas flow refers to an inert gas flow that does not participate in the reaction, such as nitrogen gas flow, rare gas gas flow, etc.
[0022] In some embodiments, the flow rate of the inert gas flow may be 10-500 mL / min, such as 30 mL / min, 100 mL / min, etc.
[0023] In the present invention, the heating rate is preferably 30-100°C / min, such as 50°C / min, 100°C / min, etc.
[0024] In some embodiments, the catalytic gasification time may be 30-480 minutes.
[0025] In the present invention, the temperature used for adsorption and capture of mercuric chloride is greater than the volatilization temperature of mercuric chloride powder, 140°C, so that gaseous mercuric chloride and (chlorinated) defective carbon carriers can form chemical adsorption, thereby forming a monolayer of dispersed mercuric chloride on the surface of (chlorinated) defective carbon carriers, and the saturated adsorption amount of mercuric chloride of (chlorinated) defective carbon carriers is much higher than the content of adsorbed and captured mercuric chloride, which can ensure that mercuric chloride has sufficient anchoring points without agglomeration. In some embodiments, the adsorption and capture temperature is greater than 140°C, and further, may not exceed 250°C, specifically 150-250°C, such as 150°C, 180°C, etc.
[0026] The invention also provides a single-atom mercury catalyst prepared by the method.
[0027] The existing waste mercury catalyst treatment technology has the problem that the recovery process is complicated and the carbon material after recovery and treatment cannot be used in a high-value manner. The present invention provides a method for preparing a single-atom mercury catalyst using waste mercury catalyst as a raw material. The waste mercury catalyst is used as a raw material and a catalytic gasification-defect capture method is adopted to obtain a high-performance single-atom mercury catalyst in one step. At the same time, the carbon carrier after catalytic mercury extraction is crushed, bonded and formed and catalytically carbonized to obtain a chlorinated defect carbon carrier, which is reused as a carrier of the single-atom mercury catalyst, thereby realizing the recycling of all waste mercury catalyst materials.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] 1. The present invention uses waste mercury catalyst as raw material to regenerate and prepare high-performance single-atom mercury catalyst in one step. The process is simple and the waste catalyst treatment and new catalyst preparation are integrated.
[0030] 2. The present invention catalytically gasifies and captures mercuric chloride in waste mercury catalysts to prepare high-performance single-atom mercury catalysts, and at the same time regenerates waste carbon carriers to obtain high-performance defective carbon carriers, thereby making full use of mercury resources and carbon resources to achieve high-value utilization of waste mercury catalyst resources.
[0031] 3. The temperature (e.g., 150-250°C) at which mercuric chloride is adsorbed and captured by chlorination-deficient activated carbon in the present invention is higher than the acetylene hydrochlorination reaction temperature of 140°C, so the prepared single-atom mercury catalyst has good thermal stability. DETAILED DESCRIPTION
[0032] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention.
[0033] Example 1
[0034] 10 kg of the dried (water content less than 3 wt%) waste mercury catalyst was weighed and mixed with 2 kg of potassium nitrate, a gasification aid, and then the mixed waste mercury catalyst was loaded into a gasification mercury extraction furnace, and 10 kg of the chlorinated defective carbon carrier was loaded into a subsequent adsorption capture furnace; then 30 mL / min of nitrogen was introduced from the gasification mercury extraction furnace, and the gasification mercury extraction furnace was heated to 300° C. at 50° C. / min and kept at a constant temperature for 2 h. The adsorption capture furnace in this stage was kept at 150° C., and then the gasification mercury extraction furnace was cooled to room temperature in a nitrogen atmosphere, and the single-atom mercury catalyst prepared in the adsorption capture furnace was taken out.
[0035] Then, the carbon material after mercury extraction in the gasification mercury extraction furnace was taken out, ground, crushed and mixed with 3 kg of activator melamine and 2 kg of binder ammonium humate in a grinder for 2 hours, and then the mixed carbon material was added with 3 kg of water for kneading and extrusion into columnar particles with a diameter of 3-5 mm, and dried at 120°C for 5 hours. Then the dried carbon material precursor was carbonized in a carbonization furnace at 850°C in an inert atmosphere for 3 hours to obtain a chlorinated defect carbon carrier material, which was used to prepare a single-atom mercury catalyst in an adsorption capture furnace.
[0036] Example 2
[0037] The difference from Example 1 is only that potassium nitrate is replaced by sodium nitrate of equal mass, and the rest is the same.
[0038] Example 3
[0039] The difference from Example 1 is only that the potassium nitrate consumption is changed to 5 kg, and all the other are the same.
[0040] Example 4
[0041] The only difference from Example 1 is that the flow rate of nitrogen introduced from the gasification mercury extraction furnace is changed to 100 mL / min, and the rest is the same.
[0042] Example 5
[0043] 20 kg of the dried (water content less than 3 wt%) waste mercury catalyst was weighed and mixed with 4 kg of potassium nitrate, a gasification aid, and then the mixed waste mercury catalyst was loaded into a gasification mercury extraction furnace, and 10 kg of a chlorinated defective carbon carrier was loaded into a subsequent adsorption capture furnace; then 30 mL / min of nitrogen was introduced from the gasification mercury extraction furnace, and the gasification mercury extraction furnace was heated to 300° C. at 50° C. / min and kept at a constant temperature for 2 h. The adsorption capture furnace in this stage was kept at 150° C., and then the gasification mercury extraction furnace was cooled to room temperature in a nitrogen atmosphere, and the single-atom mercury catalyst prepared in the adsorption capture furnace was taken out.
[0044] Then, the carbon material after mercury extraction in the gasification mercury extraction furnace was taken out, ground, crushed and mixed with 6 kg of activator melamine and 4 kg of binder ammonium humate in a grinder for 2 hours, and then the mixed carbon material was added with 6 kg of water for kneading and extrusion into columnar particles with a diameter of 3-5 mm, and dried at 120°C for 5 hours. Then the dried carbon material precursor was carbonized in a carbonization furnace at 850°C in an inert atmosphere for 3 hours to obtain a chlorinated defect carbon carrier material, which was used to prepare a single-atom mercury catalyst in an adsorption capture furnace.
[0045] Example 6
[0046] The only difference from Example 1 is that the final temperature of the gasification mercury extraction furnace is changed from 300° C. to 350° C., and the rest are the same.
[0047] Example 7
[0048] The only difference from Example 1 is that the temperature of the adsorption capture furnace is changed from 150° C. to 180° C., and the rest are the same.
[0049] Example 8
[0050] The only difference from Example 1 is that the heating rate of the gasification mercury extraction furnace is changed from 50° C. / min to 100° C. / min, and the rest are the same.
[0051] Example 9
[0052] 10 kg of the dried (water content less than 3 wt%) waste mercury catalyst was weighed and mixed with 2 kg of potassium nitrate, a gasification aid, and then the mixed waste mercury catalyst was loaded into a gasification mercury extraction furnace, and 10 kg of the chlorinated defective carbon carrier was loaded into a subsequent adsorption capture furnace; then 30 mL / min of nitrogen was introduced from the gasification mercury extraction furnace, and the gasification mercury extraction furnace was heated to 300° C. at 50° C. / min and kept at a constant temperature for 2 h. The adsorption capture furnace in this stage was kept at 150° C., and then the gasification mercury extraction furnace was cooled to room temperature in a nitrogen atmosphere, and the single-atom mercury catalyst prepared in the adsorption capture furnace was taken out.
[0053] Then, the carbon material after mercury extraction in the gasification mercury extraction furnace was taken out, ground, crushed and mixed with 6 kg of activator melamine and 4 kg of binder ammonium humate in a grinder for 2 hours, and then the mixed carbon material was added with 4 kg of water for kneading and extrusion into columnar particles with a diameter of 3-5 mm, and dried at 120°C for 5 hours. Then the dried carbon material precursor was carbonized in a carbonization furnace at 850°C in an inert atmosphere for 3 hours to obtain a chlorinated defect carbon carrier material, which was used to prepare a single-atom mercury catalyst in an adsorption capture furnace.
[0054] Example 10
[0055] The only difference from Example 1 is that the ammonium humate is replaced by an equal mass of phenolic resin, and the rest is the same.
[0056] Comparative Example 1
[0057] Weigh 10kg of activated carbon, add 30L of 30% nitric acid solution by volume, treat at 90℃ for 5h, wash with deionized water, and then place in a drying furnace at 120℃ for 12h; the dried activated carbon is then placed in a tubular furnace for deoxygenation and defect treatment. Under nitrogen conditions, the temperature is raised from room temperature to 800℃ in 4 hours, kept constant for 10min, and naturally cooled to room temperature to take out the sample, thus obtaining defect-rich activated carbon. Accurately weigh 0.2kg of mercuric chloride, dissolve it with 7L of 0.1mol / L hydrochloric acid solution, and after the mercuric chloride is completely dissolved, load it onto 10kg of defective activated carbon by spraying, and immerse it at room temperature for 12h. The impregnated mercuric chloride catalyst is placed in a drying furnace for drying, the drying temperature is set to 100℃, and dried for 8h to remove the moisture in the catalyst, thus obtaining a single-atom mercury catalyst with a mercuric chloride content of 2%.
[0058] Comparative Example 2
[0059] Weigh 2kg of coal-based carbon powder and 0.5kg of sucralose and dissolve them in 1.6L of deionized water. After the sucralose is completely dissolved, gradually add it to the mixture of carbon powder and metal nitrate. After stirring and kneading, place it at room temperature for 10 hours. The obtained sample is sent to the extruder for pressure extrusion to obtain a columnar carbon with a diameter of 1.5mm. It is placed at room temperature for 10 hours, and then dried at 110℃ for 8 hours to remove excess moisture. The obtained sample is then sent to a rotary kiln, and under nitrogen conditions, the temperature is raised to 800℃ at a heating rate of 5℃ / min, and the temperature is kept constant for 5 hours for deep carbonization treatment. Cool naturally to room temperature to obtain chlorine-doped defective activated carbon. Accurately weigh 0.021kg of mercuric chloride and dissolve it in 0.8L of 1mol / L hydrochloric acid solution. Weigh 1 kg of the above-mentioned chlorine-doped defective activated carbon and put it into the impregnation tank for use. After the mercuric chloride is completely dissolved, add the mercuric chloride impregnation solution into the impregnation tank and stir it appropriately to make it impregnated evenly. Impregnate for 18 hours at room temperature and then dry it at 110°C for 12 hours to obtain an ultra-low mercury catalyst with a mercuric chloride mass fraction of 2wt%.
[0060] Comparative Example 3
[0061] Weigh 10 kg of the dried (water content less than 3 wt%) waste mercury catalyst and directly load it into the gasification mercury stripping furnace, and load 10 kg of the chlorinated defective carbon carrier into the subsequent adsorption capture furnace; then introduce 30 mL / min of nitrogen from the gasification mercury stripping furnace, heat the gasification mercury stripping furnace to 300 ° C at 50 ° C / min and keep the temperature constant for 2 hours. The adsorption capture furnace in this stage is kept at 150 ° C. After that, the gasification mercury stripping furnace is cooled to room temperature in a nitrogen atmosphere, and the mercury catalyst prepared in the adsorption capture furnace is taken out.
[0062] Then, the carbon material after mercury extraction in the gasification mercury extraction furnace was taken out, ground, crushed and mixed with 3 kg of activator melamine and 2 kg of binder ammonium humate in a grinder for 2 hours, and then the mixed carbon material was added with 3 kg of water for kneading and extrusion into columnar particles with a diameter of 3-5 mm, and dried at 120°C for 5 hours. Then the dried carbon material precursor was carbonized in a carbonization furnace at 850°C in an inert atmosphere for 3 hours to obtain a chlorinated defect carbon carrier material, which was used to prepare a single-atom mercury catalyst in an adsorption capture furnace.
[0063] Comparative Example 4
[0064] 10 kg of the dried (water content less than 3 wt%) waste mercury catalyst was weighed and mixed with 2 kg of potassium nitrate, a gasification aid, and then the mixed waste mercury catalyst was loaded into a gasification mercury extraction furnace, and 10 kg of untreated 3-5 mm columnar coal-based activated carbon was loaded into a subsequent adsorption capture furnace; then 30 mL / min of nitrogen was introduced from the gasification mercury extraction furnace, and the gasification mercury extraction furnace was heated to 300° C. at 50° C. / min and kept at a constant temperature for 2 hours. The adsorption capture furnace in this stage was kept at 150° C., and then the gasification mercury extraction furnace was cooled to room temperature in a nitrogen atmosphere, and the mercury catalyst prepared in the adsorption capture furnace was taken out.
[0065] Comparative Example 5
[0066] 10 kg of coal-based carbon powder, 3 kg of activator melamine and 2 kg of binder ammonium humate were ground, crushed and mixed in a grinder for 2 hours, and then the mixed carbon material was added with 3 kg of water for kneading and extrusion into columnar particles with a diameter of 3-5 mm, and dried at 120°C for 5 hours. Then the dried carbon material precursor was carbonized in a carbonization furnace at 850°C in an inert atmosphere for 3 hours to obtain a carbon carrier material prepared with fresh coal-based carbon powder as raw material, which was used to prepare a single-atom mercury catalyst in an adsorption capture furnace.
[0067] Then, 10 kg of the dried (water content less than 3 wt%) waste mercury catalyst was weighed and mixed with 2 kg of potassium nitrate, a gasification aid, and then the mixed waste mercury catalyst was loaded into a gasification mercury extraction furnace, and 10 kg of a carbon carrier material prepared with fresh coal-based carbon powder as a raw material was loaded into a subsequent adsorption capture furnace; then, 30 mL / min of nitrogen was introduced from the gasification mercury extraction furnace, and the gasification mercury extraction furnace was heated to 300° C. at 50° C. / min and kept at a constant temperature for 2 h. During this stage, the adsorption capture furnace was kept at 150° C., and then the gasification mercury extraction furnace was cooled to room temperature in a nitrogen atmosphere, and the single-atom mercury catalyst prepared in the adsorption capture furnace was taken out.
[0068] Comparative Example 6
[0069] The only difference from Example 1 is that the heating rate of the gasification mercury extraction furnace is changed from 50° C. / min to 5° C. / min, and the rest are the same.
[0070] The mercury catalysts prepared in the examples and comparative examples were heated at 140°C and an acetylene space velocity of 30 h -1 The catalytic performance was evaluated under the conditions of V(HCl) / V(C2H2)=1.1:1, and the obtained data are listed in Table 1.
[0071] Table 1
[0072] sample Acetylene conversion rate (%) Vinyl chloride selectivity (%) Example 1 99.6 >99 Example 2 96.5 >99 Example 3 98.1 >99 Example 4 99.8 >99 Example 5 99.4 >99 Example 6 98.4 >99 Example 7 99.3 >99 Example 8 99.7 >99 Example 9 97.6 >99 Example 10 99.6 >99 Comparative Example 1 93.2 >99 Comparative Example 2 95.3 >99 Comparative Example 3 30.6 >99 Comparative Example 4 43.2 >99 Comparative Example 5 95.8 >99 Comparative Example 6 94.3 >99
[0073] As can be seen from Table 1, from the data of acetylene conversion rates of Comparative Example 1, Comparative Example 2 and Examples 1-10, it can be seen that the activity of the single-atom mercury catalyst prepared using waste mercury catalyst as raw material in Examples 1-10 has reached or exceeded the activity of the single-atom catalyst prepared using fresh mercuric chloride and activated carbon as carbon carrier.
[0074] By comparing Example 1 with Example 2, Example 3, Example 4, Example 5, Example 6, and Example 7, it can be found that changing the type and amount of the gasification aid, the flow rate of the inert gas flow during mercury extraction gasification, the ratio of the waste mercury catalyst to the defective activated carbon, the final temperature of the gasification mercury extraction furnace, and the adsorption capture temperature will have a certain effect on the acetylene conversion rate of the final mercury catalyst.
[0075] By comparing Example 1, Example 8 and Comparative Example 6, it can be found that changing the heating rate of the gasification mercury extraction furnace will affect the acetylene conversion rate of the final mercury catalyst, and when the heating rate is lower than 30°C / min, the acetylene conversion rate decreases more significantly.
[0076] By comparing Example 1 with Example 9 and Example 10, it can be found that changing the proportion of waste carbon and the binder when preparing chlorinated defective activated carbon will have a certain effect on the acetylene conversion rate of the final mercury catalyst.
[0077] By comparing Examples 1-10 and Comparative Example 3, it can be found that when no gasification aid is added during the mercury extraction process, the acetylene conversion rate of the catalyst is significantly reduced. This is because without the gasification aid, the mercuric chloride in the waste mercury catalyst cannot be completely extracted.
[0078] By comparing Examples 1-10 and Comparative Example 4, it can be found that when ordinary coal-based activated carbon is used instead of chloride-defect activated carbon for adsorption and capture, the acetylene conversion rate of the catalyst is significantly reduced. This is because ordinary coal-based activated carbon does not have a large number of defects and cannot effectively adsorb and capture the emitted mercuric chloride.
[0079] By comparing Examples 1-10 and Comparative Example 5, it can be found that when preparing chlorination-deficient activated carbon, instead of using waste catalyst activated carbon, new coal-based carbon powder is used, and the acetylene of the catalyst is reduced to a certain extent, indicating that using activated carbon materials extracted from waste mercury catalysts as raw materials for preparing chlorination-deficient activated carbon can improve the acetylene conversion rate of the catalyst. This may be because the additives remaining in the activated carbon materials after the waste mercury catalysts are extracted promote the activation of the carbon materials.
[0080] In addition, it should be understood that after reading the above description of the present invention, those skilled in the art may make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the claims attached to this application.
Claims
1. A method for preparing a single-atom mercury catalyst using waste mercury catalyst as raw material, characterized in that: include: The waste mercury catalyst is mixed with a mercuric chloride gasification aid, and then heated to 300-350°C in an inert gas flow for catalytic gasification, and the mercuric chloride in the catalytic gasification tail gas is adsorbed and captured by a defective carbon carrier to obtain a single-atom mercury catalyst; the heating rate is 30-100°C / min; The mercuric chloride gasification aid includes at least one of potassium nitrate, sodium nitrate, barium nitrate, zinc nitrate and cerium nitrate.
2. The method according to claim 1, characterized in that The water content of the spent mercury catalyst is less than 3 wt %.
3. The method according to claim 1 or 2, characterized in that: The mass ratio of the mercuric chloride gasification aid to the waste mercury catalyst is 1-5:10, preferably 2:
10.
4. The method according to claim 1, characterized in that: The defective carbon support comprises a chlorinated defective carbon support; The preparation method of the chlorinated defective carbon carrier comprises: mixing the solid product of the catalytic gasification with an activator and a binder, grinding and crushing the solid product, kneading and molding the solid product, drying the solid product, and carbonizing the solid product in an inert atmosphere to obtain the chlorinated defective carbon carrier.
5. The method according to claim 4, characterized in that In the preparation method of the chlorinated defective carbon support: The activator comprises at least one of melamine, dicyandiamide, urea and cyanuric acid; The mass ratio of the activator to the waste mercury catalyst is 1-5:10; The binder includes at least one of gelatinized starch, humate, and phenolic resin; The mass ratio of the binder to the waste mercury catalyst is 1-5:10; The carbonization temperature is 800-900°C, preferably 850°C, and the time is 2-4h, preferably 3h.
6. The method according to claim 1, 4 or 5, characterized in that: The mass ratio of the defective carbon support to the waste mercury catalyst is 1:1-10.
7. The method according to claim 1, characterized in that The flow rate of the inert gas flow is 10-500 mL / min.
8. The method according to claim 1, characterized in that The catalytic gasification time is 30-480 minutes.
9. The method according to claim 1, characterized in that: The temperature of the adsorption capture is 150-250°C.
10. The single-atom mercury catalyst prepared by the method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Method for recycling waste mercury catalyst from polyvinyl chloride production based on calcium carbide method
CN106673055A
High-stability ultralow-mercury catalyst, and preparation method and application thereof
CN110227507A
Monoatomic mercury catalyst, and preparation method and application thereof
CN110227508A
Sorbents for Removal of Mercury From Flue Gas Cross Reference To Related Applications