Preparation method of special-shaped salt-based ceramic core
By using a mixture of sodium chloride powder and ceramic powder, along with a specific binder, combined with supercritical CO2 extraction and controlled sintering temperature, a high-precision, smooth-surfaced irregularly shaped salt-based ceramic core was prepared. This solved the problem of separation between the ceramic core and the irregularly shaped casting, ensuring that the casting is not damaged.
Patent Information
- Application Number
- CN202410950191.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-22
AI Technical Summary
Existing technologies struggle to produce ceramic cores with high precision, smooth inner surfaces, and easy separation from irregularly shaped castings, while also ensuring that the castings are not damaged during the casting process.
A mixed powder of sodium chloride powder and ceramic powder with a mass ratio of (65-75):(25-35) was used, combined with a specific binder and supercritical CO2 extraction technology, and irregularly shaped salt-based ceramic cores were prepared by medium-pressure injection molding and controlled sintering temperature.
It achieves high precision and smooth inner surface of irregularly shaped salt-based ceramic cores, and is easy to peel off after casting preparation, avoiding casting damage and maintaining shape stability during the casting process.
Abstract
Description
Technical Field
[0001] The invention relates to the field of ceramic cores, and in particular to the field of a method for preparing a special-shaped salt-based ceramic core. Background Art
[0002] The ceramic core serves as a transition body for forming the casting cavity, forming the inner cavity structure of the casting, and together with the outer mold and the mold shell, ensures the dimensional accuracy requirements of the casting for the cavity; with the popularization and development of new energy vehicles in my country, the demand for internal cooling channels in aluminum parts of the automotive industry has increased.
[0003] The ceramic core required for the preparation of special-shaped castings with complex structures must meet the requirements of precision and smooth contact surface with the casting, and the ceramic core can be easily separated from the special-shaped casting without causing damage to the special-shaped casting.
[0004] Therefore, how to invent a special-shaped ceramic core with high precision, smooth inner surface and easy separation from the special-shaped casting after processing the casting has become a difficult problem that urgently needs to be solved in this field. Summary of the invention
[0005] The purpose of the present invention is to provide a method for preparing a special-shaped salt-based ceramic core, so that the prepared special-shaped salt-based ceramic core has high precision and a smooth inner surface, and the special-shaped salt-based ceramic core can be easily partially or decomposed when it comes into contact with water after preparing a special-shaped casting, and then the special-shaped salt-based ceramic core can be easily separated from the special-shaped casting.
[0006] The present invention provides a method for preparing a special-shaped salt-based ceramic core, comprising the following steps:
[0007] Prepare a mixed powder, wherein the mixed powder comprises sodium chloride powder and ceramic powder in a mass ratio of (65-75):(25-35);
[0008] Prepare a mixed mud material, mix and knead the mixed powder to obtain a mixed mud material; the mixed mud material includes a first binder and a second binder;
[0009] The mixed mud material is directly or granulated by medium pressure injection molding to obtain a ceramic green body;
[0010] Debinding the ceramic green body to obtain a final ceramic green body; the debinding process includes primary debinding and secondary debinding;
[0011] The final ceramic body is sintered to obtain the special-shaped salt-based ceramic core; the sintering temperature is 900-950°C.
[0012] The beneficial effect of the present invention over the prior art is that, by virtue of the mixed powder comprising sodium chloride powder and ceramic powder in a mass ratio of (65-75):(25-35), the special-shaped salt-based ceramic core contains sodium chloride, and the sodium chloride content is high, so that the special-shaped salt-based ceramic core is partially or completely decomposed when it comes into contact with water, and at the same time, the strength of the special-shaped salt-based ceramic core meets the application environment of gravity casting and pressure casting, and does not deform or crack during the casting process;
[0013] The mixed powder is mixed and kneaded with a binder to obtain a mixed mud material; the first binder and the second binder are included to achieve high strength of the ceramic green body, and at the same time facilitate smooth debinding of the ceramic green body, and the ceramic green body does not deform or damage during the debinding process, thereby facilitating the improvement of the precision of the special-shaped salt-based ceramic core and achieving the smoothness of the inner surface of the special-shaped salt-based ceramic core;
[0014] The sintering temperature is 900-950° C., which is relatively high, and is conducive to achieving a higher ceramic structure strength of the sintered ceramic powder in the special-shaped salt-based ceramic core, and does not affect the internal precision and internal surface smoothness of the ceramic core.
[0015] Furthermore, the ceramic powder includes a first ceramic powder and a second ceramic powder in a mass ratio of (40-60): (60-40);
[0016] The first ceramic powder includes one or both of mullite and alumina; the second powder includes one or both of zircon powder and quartz powder.
[0017] The beneficial effect of adopting the previous step is that the ceramic powder is helpful to improve the strength of the prepared special-shaped salt-based ceramic core.
[0018] Furthermore, the specific process of the mixed powder and mixed kneading is as follows:
[0019] The mixed powder and the binder system are weighed in a mass ratio of (80-90): (20-10), added into a mixing device in 2-5 portions for mixing and stirring at a temperature of 90-120° C. and a rotation speed of 20-60 rpm / min to obtain a mixed mud.
[0020] The beneficial effect of adopting the previous step is that the mixed powder and the binder system material are mixed evenly; the temperature of 90-120°C is conducive to the liquefaction of the first binder and to the good dispersion effect after the first binder is liquefied; at the same time, the problem of sodium chloride dissolution caused by moisture absorption during the mud preparation process is avoided.
[0021] Furthermore, the first binder includes one of microcrystalline wax and rosin;
[0022] The second binder includes one or more of cocamide, dioctyl phthalate, and dioctyl adipate;
[0023] The mass ratio of the first binder to the second binder is (70-80):(26-18.5).
[0024] The beneficial effect of adopting the previous step is that the first binder includes one of microcrystalline wax and rosin, which is conducive to improving the strength of the special-shaped salt-based ceramic core, and at the same time, the first binder is subjected to a primary debinding process by supercritical CO2 extraction, while avoiding deformation of the ceramic green body during the primary debinding process. At the same time, due to the formation of a number of through holes in the ceramic green body by the discharge of the first binder, it is conducive to the smooth discharge of the subsequent second binder during the secondary debinding process; the first binder is conducive to avoiding the problem of moisture absorption of the ceramic green body, thereby avoiding the problem of reduced strength or deformation of the ceramic green body.
[0025] Furthermore, the mixed mud material is cooled and pelletized to obtain ceramic feed material, and the ceramic feed material is used for medium pressure injection molding to obtain a ceramic green body;
[0026] The mixed mud is cooled and pelletized under negative pressure.
[0027] Furthermore, the medium pressure injection molding process is as follows: the mixed mud material is added directly or after granulation into a medium pressure injection molding device, the injection temperature is set to 85-100° C., and the injection rate is set to 2-8 cm / s to obtain a ceramic green body;
[0028] Preferably, the medium-pressure injection molding equipment is in a state of slight negative pressure; air is extracted from the medium-pressure injection molding equipment by a vacuum pump, so that the medium-pressure injection molding equipment is in a state of slight negative pressure.
[0029] The beneficial effect of adopting the previous step is that near-net-size molding can be achieved without any processing, and the obtained ceramic green body has high precision, thereby achieving high precision of the prepared special-shaped salt-based ceramic core.
[0030] Furthermore, the first-level debinding process includes the following steps:
[0031] The ceramic green body is extracted by supercritical CO2, the extraction pressure of the supercritical CO2 fluid is 15-35MPa, the extraction temperature is 60-80°C, the extraction time is 2-4h, the extraction flow rate is 0.5-1.5L / h, and a primary ceramic green body is obtained.
[0032] The beneficial effect of adopting the previous step is that the first binder is discharged from the ceramic green body by extracting the ceramic green body with supercritical CO2, while avoiding deformation of the ceramic green body during the primary debinding process and avoiding the problem of increased roughness on the surface of the ceramic green body when the ceramic green body is debinded thermally without generating a plurality of through holes inside. In addition, a plurality of through holes are formed in the ceramic green body during the discharge process of the first binder, which is conducive to the smooth discharge of the subsequent second binder in the secondary debinding process, thereby avoiding the problem of deformation or damage of the ceramic green body during the entire debinding process.
[0033] Furthermore, the secondary debinding process comprises the following steps:
[0034] The first-class ceramic body is heated to remove binder, and the temperature of the first-class ceramic body is raised from room temperature to 90-110°C at a heating rate of 8-9°C / min; from 90-110°C to 350-450°C at a heating rate of 0.3-0.6°C / min; and the heat preservation time at 350-450°C is 3-5h.
[0035] The beneficial effect of adopting the previous step is that by heating the first-level ceramic body from room temperature to 90-110°C at a heating rate of 8-9°C / min, it is beneficial to achieve rapid volatilization of small molecular weight volatiles remaining in the first-level ceramic body on the basis of the channels generated by the discharge of the first binder, and it is beneficial to expand the pore size to facilitate the subsequent debinding of large molecular weight volatiles; by heating from 90-110°C to 350-450°C at a heating rate of 0.3-0.6°C / min, slow heating is achieved, organic large molecular volatiles are slowly decomposed, and slowly volatilize on the basis of the channels generated by the early debinding, thereby avoiding problems such as deformation or cracking of the ceramic green body during the debinding process.
[0036] Furthermore, the sintering of the final ceramic body comprises the following steps:
[0037] The ultimate ceramic body is heated to 750-850°C at a heating rate of 0.3-0.6°C / min, and kept at 750-850°C for 0.5-0.8h; then the temperature is raised from 750-850°C to 900-950°C, and kept at 900-950°C for 1.2-3.5h, and the ultimate ceramic body is sintered in a rotating state;
[0038] Preferably, when the temperature during sintering is ≤850°C, the rotation speed of the final ceramic body is 8-15 rpm;
[0039] When the temperature during the sintering process is greater than 850°C, the ultimate ceramic body rotation speed is 3-8 revolutions per minute.
[0040] The beneficial effect of adopting the previous step is that the heating rate is helpful to avoid the problem of excessive local heating, thereby avoiding the problem of deformation of the special-shaped salt-based ceramic core caused by the early softening and strong fluidity of the local sodium chloride powder;
[0041] By sintering the ultimate ceramic blank in a rotating state, it is beneficial to realize that when the sodium chloride softens at a high temperature during the sintering process, the sodium chloride will have a tendency to flow toward the outer surface of the special-shaped salt-based ceramic core under the action of centrifugal force, thereby avoiding the problem that the sodium chloride may overflow slightly or in small amounts from the inner surface of the special-shaped salt-based ceramic core when the temperature is greater than 850° C., thereby avoiding the problem that the inner surface of the special-shaped salt-based ceramic core is not smooth;
[0042] When the temperature during the sintering process is ≤850°C, the rotation speed of the ultimate ceramic body is 8-15 rpm; when the temperature during the sintering process is >850°C, the rotation speed of the ultimate ceramic body is 3-8 rpm, so that when the softening or viscosity of sodium chloride is different at different temperatures, the sodium chloride is subjected to different centrifugal forces. As the temperature rises, the softening degree or viscosity of sodium chloride increases, the speed is controlled to decrease, and the centrifugal force is reduced, thereby avoiding the problem of uneven heating inside the special-shaped salt-based ceramic core caused by more sodium chloride flowing to the outer surface of the special-shaped salt-based ceramic core. DETAILED DESCRIPTION
[0043] In order to better understand the technical solution of the present invention, the present invention is further described below in conjunction with specific embodiments.
[0044] Embodiment 1:
[0045] This embodiment provides a method for preparing a special-shaped salt-based ceramic core, comprising the following steps:
[0046] Prepare a mixed powder, the mixed powder comprising sodium chloride powder and ceramic powder in a mass ratio of 70:30; the ceramic powder comprises a first ceramic powder and a second ceramic powder in a mass ratio of 50:50;
[0047] The first ceramic powder includes alumina; the second powder includes zircon powder.
[0048] Prepare a mixed mud material, mix and knead the mixed powder to obtain a mixed mud material; the specific process of the mixed powder and the mixed kneading is as follows:
[0049] The mixed powder and the binder system are weighed in a mass ratio of 85:15, added into a mixing device in four portions for mixing and stirring at a temperature of 90-120° C. and a rotation speed of 20-60 rpm / min to obtain a mixed mud.
[0050] The invention comprises a first binder and a second binder; the first binder is microcrystalline wax;
[0051] The second adhesive package is dioctyl phthalate;
[0052] The mass ratio of the first binder to the second binder is 75:22.
[0053] The mixed clay material is cooled and pelletized to obtain ceramic feed material, and the ceramic feed material is used for medium-pressure injection molding to obtain a ceramic green body; the mixed clay material is cooled and pelletized in a negative pressure environment.
[0054] The mixed mud is directly or granulated by medium pressure injection molding to obtain a ceramic green body; the medium pressure injection molding process is as follows: the mixed mud is added to the medium pressure injection molding equipment after granulation, the injection temperature is set to 92°C, and the injection rate is 5 cm / s to obtain a ceramic green body; the medium pressure injection molding equipment is in a slightly negative pressure state; and air is evacuated from the medium pressure injection molding equipment by a vacuum pump to achieve a slightly negative pressure state in the medium pressure injection molding equipment.
[0055] Debinding the ceramic green body to obtain a final ceramic green body; the debinding process includes primary debinding and secondary debinding;
[0056] The primary debinding process comprises the following steps: extracting the ceramic green body with supercritical CO2, wherein the extraction pressure of the supercritical CO2 fluid is 25MPa, the extraction temperature is 70°C, the extraction time is 3h, and the extraction flow rate is 1L / h to obtain a primary ceramic green body.
[0057] The secondary debinding process comprises the following steps: heating the primary ceramic body for debinding, heating the primary ceramic body from room temperature to 100°C at a heating rate of 8.5°C / min; heating from 100°C to 400°C at a heating rate of 0.45°C / min; and keeping the temperature at 400°C for 4 hours.
[0058] The final ceramic body is sintered to obtain the special-shaped salt-based ceramic core; the sintering temperature is 920° C. The final ceramic body is sintered including the following steps:
[0059] The ultimate ceramic body is heated to 800°C at a heating rate of 0.45°C / min, and kept at 800°C for 0.65h; then the temperature is raised from 800°C to 920°C, and kept at 920°C for 2.3h, and the ultimate ceramic body is sintered in a rotating state;
[0060] When the temperature during sintering is ≤850°C, the rotation speed of the final ceramic body is 12 rpm;
[0061] When the temperature during the sintering process is greater than 850°C, the ultimate ceramic body rotation speed is 6 revolutions / min.
[0062] Embodiment 2:
[0063] The same contents as those in Example 1 are not described in detail here. The differences between this embodiment and Example 1 are as follows:
[0064] This embodiment provides a method for preparing a special-shaped salt-based ceramic core, wherein the mixed powder includes sodium chloride powder and ceramic powder in a mass ratio of 73:28; the ceramic powder includes a first ceramic powder and a second ceramic powder in a mass ratio of 58:42;
[0065] The first ceramic powder includes mullite; and the second powder includes quartz powder.
[0066] The mixed powder and the binder system were weighed in a mass ratio of 88:12, added into a mixing device in four portions for mixing and stirring at a temperature of 95° C. and a rotation speed of 30 rpm / min to obtain a mixed mud material.
[0067] The first binder is rosin; the second binder is cocamide and dioctyl phthalate;
[0068] The mass ratio of the first binder to the second binder is 72:23.
[0069] The mixed mud material was granulated and then added into a medium pressure injection molding device, and the injection molding temperature was set at 88° C. and the injection molding rate was set at 6 cm / s to obtain a ceramic green body.
[0070] The ceramic green body is extracted with supercritical CO2, the extraction pressure of the supercritical CO2 fluid is 18MPa, the extraction temperature is 65°C, the extraction time is 2.5h, the extraction flow rate is 0.8L / h, and a primary ceramic green body is obtained.
[0071] The first-level ceramic body is heated to debind, and the temperature of the first-level ceramic body is raised from room temperature to 95°C at a heating rate of 8.2°C / min; the temperature is raised from 95°C to 380°C at a heating rate of 0.35°C / min; and the temperature is kept at 380°C for 4.5 hours.
[0072] The sintering temperature is 940°C;
[0073] The ultimate ceramic body is heated to 780°C at a heating rate of 0.35°C / min, and kept at 780°C for 0.6h; then the temperature is raised from 780°C to 940°C, and kept at 940°C for 3h, and the ultimate ceramic body is sintered in a rotating state;
[0074] When the temperature during sintering is ≤850°C, the rotation speed of the final ceramic body is 14 rpm;
[0075] When the temperature during the sintering process is greater than 850°C, the ultimate ceramic body rotation speed is 7 revolutions per minute.
[0076] Embodiment 3:
[0077] The same contents as those in Example 1 are not described in detail here. The differences between this embodiment and Example 1 are as follows:
[0078] This embodiment provides a method for preparing a special-shaped salt-based ceramic core, wherein the mixed powder includes sodium chloride powder and ceramic powder in a mass ratio of 68:32; the ceramic powder includes a first ceramic powder and a second ceramic powder in a mass ratio of 43:57;
[0079] The first ceramic powder includes mullite; and the second powder includes quartz powder.
[0080] The mixed powder and the binder system were weighed in a mass ratio of 82:18, added into a mixing device for three times for mixing and stirring at a temperature of 115° C. and a rotation speed of 55 rpm / min to obtain a mixed mud.
[0081] The first binder includes rosin; the second binder includes dioctyl phthalate and dioctyl adipate;
[0082] The mass ratio of the first binder to the second binder is 78:20.
[0083] The mixed mud material was granulated and then added into a medium pressure injection molding device, and the injection molding temperature was set at 96° C. and the injection molding speed was set at 3 cm / s to obtain a ceramic green body.
[0084] The ceramic green body was extracted with supercritical CO2, the extraction pressure of the supercritical CO2 fluid was 30MPa, the extraction temperature was 78°C, the extraction time was 3.5h, the extraction flow rate was 1.3L / h, and a primary ceramic green body was obtained.
[0085] The first-level ceramic body is heated to debind, and the temperature of the first-level ceramic body is raised from room temperature to 105°C at a heating rate of 8.8°C / min; the temperature is raised from 105°C to 430°C at a heating rate of 0.55°C / min; and the temperature is kept at 430°C for 3.5 hours.
[0086] The sintering temperature is 910°C;
[0087] The ultimate ceramic body is heated to 830° C. at a heating rate of 0.56° C. / min, and kept at 830° C. for 0.75 h; then the temperature is raised from 830° C. to 910° C., and kept at 910° C. for 1.8 h, and the ultimate ceramic body is sintered in a rotating state;
[0088] When the temperature during sintering is ≤850°C, the rotation speed of the final ceramic body is 10 rpm;
[0089] When the temperature during the sintering process is greater than 850°C, the ultimate ceramic body rotation speed is 4 revolutions per minute.
[0090] The above description is only a preferred embodiment of the present application and an explanation of the technical principles used. Those skilled in the art should understand that the scope of the invention involved in the present application is not limited to the technical solution formed by a specific combination of the above technical features, but should also cover other technical solutions formed by any combination of the above technical features or their equivalent features without departing from the inventive concept. For example, the above features have similar functions to those disclosed in the present application (but not limited to).
Claims
1. A method for preparing a special-shaped salt-based ceramic core, characterized in that: The following steps are involved: Prepare a mixed powder, wherein the mixed powder comprises sodium chloride powder and ceramic powder in a mass ratio of (65-75):(25-35); Preparing a mixed mud material, mixing and kneading the mixed powder with a bonding system material to obtain a mixed mud material; the bonding system material includes a first bonding agent and a second bonding agent; The mixed mud material is directly or granulated by medium pressure injection molding to obtain a ceramic green body; Debinding the ceramic green body to obtain a final ceramic green body; the debinding process includes primary debinding and secondary debinding; The final ceramic body is sintered to obtain the special-shaped salt-based ceramic core; the sintering temperature is 900-950°C.
2. The method for preparing a special-shaped salt-based ceramic core according to claim 1, characterized in that: The ceramic powder comprises a first ceramic powder and a second ceramic powder in a mass ratio of (40-60):(60-40); The first ceramic powder includes one or both of mullite and alumina; the second powder includes one or both of zircon powder and quartz powder.
3. The method for preparing a special-shaped salt-based ceramic core according to claim 1, characterized in that: The specific process of mixing and kneading the mixed powder and the bonding system material is as follows: The mixed powder and the binder system material are weighed in a mass ratio of (80-90): (20-10), added into a mixing device in 2-5 times for mixing and stirring at a temperature of 90-120° C. and a rotation speed of 20-60 rpm / min to obtain a mixed mud material.
4. The method for preparing a special-shaped salt-based ceramic core according to claim 1, characterized in that: The first binder includes one of microcrystalline wax and rosin; The second binder includes one or more of cocamide, dioctyl phthalate, and dioctyl adipate; The mass ratio of the first binder to the second binder is (70-80):(26-18.5).
5. The method for preparing a special-shaped salt-based ceramic core according to claim 1, characterized in that: The invention also includes stearic acid and polyacrylamide; The mass ratio of the first binder, the second binder, stearic acid and polyacrylamide is (70-80): (26-18.5): (1-3): (0.5-1).
6. The method for preparing a special-shaped salt-based ceramic core according to claim 1, characterized in that: The mixed mud material is cooled and pelletized to obtain ceramic feed material, and the ceramic feed material is used for medium pressure injection molding to obtain a ceramic green body; The mixed mud is cooled and pelletized under negative pressure.
7. The method for preparing a special-shaped salt-based ceramic core according to claim 1, characterized in that: The medium pressure injection molding process is as follows: the mixed mud material is added directly or after granulation into the medium pressure injection molding equipment, the injection molding temperature is set to 85-100° C., the injection molding rate is set to 2-8 cm / s, and a ceramic green body is obtained.
8. The method for preparing a special-shaped salt-based ceramic core according to claim 1, characterized in that: The primary debinding process comprises the following steps: The ceramic green body is extracted by supercritical CO2, the extraction pressure of the supercritical CO2 fluid is 15-35MPa, the extraction temperature is 60-80°C, the extraction time is 2-4h, the extraction flow rate is 0.5-1.5L / h, and a primary ceramic green body is obtained.
9. The method for preparing a special-shaped salt-based ceramic core according to claim 1, characterized in that: The secondary debinding process comprises the following steps: The first-class ceramic body is heated to remove binder, and the temperature of the first-class ceramic body is raised from room temperature to 90-110°C at a heating rate of 8-9°C / min; from 90-110°C to 350-450°C at a heating rate of 0.3-0.6°C / min; and the heat preservation time at 350-450°C is 3-5h.
10. The method for preparing a special-shaped salt-based ceramic core according to claim 1, characterized in that: The sintering of the final ceramic body comprises the following steps: The ultimate ceramic body is heated to 750-850°C at a heating rate of 0.3-0.6°C / min, and kept at 750-850°C for 0.5-0.8h; then the temperature is raised from 750-850°C to 900-950°C, and kept at 900-950°C for 1.2-3.5h, and the ultimate ceramic body is sintered in a rotating state; Preferably, when the temperature during sintering is ≤850°C, the rotation speed of the final ceramic body is 8-15 rpm; When the temperature during the sintering process is greater than 850°C, the ultimate ceramic body rotation speed is 3-8 revolutions per minute.