Nanometer soldering paste, welding joint and preparation method of nanometer soldering paste
By directly reacting metallurgical with diamond copper by using metal nanoparticles in nano solder paste, the problem of poor surface affinity of diamond copper is solved, the welding bonding and heat dissipation performance is improved, the packaging process is simplified, and the reliability of electronic devices is improved. .
Patent Information
- Application Number
- CN202411160076.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-22
AI Technical Summary
Diamond copper has poor affinity for diamond particles on the surface with common metal materials, resulting in poor wetting of welding materials on the surface, low connection strength, poor long-term reliability, and sensitization and activation treatment will affect the packaging process and heat dissipation performance.
Nano-solder paste consisting of 30% to 60% flux, 5% to 10% nanoparticle dispersant and balance matrix solder powder. The nanoparticles are metal nanoparticles that can undergo metallurgical reaction with diamond, and the flux includes resin, Active agents, organic solvents and thixotropic agents are directly welded to the surface of diamond copper to avoid metallization.
It improves the welding bonding and reliability of diamond copper and chip, enhances heat dissipation ability, simplifies the packaging process, forms a more solid welding joint, and improves the reliability of electronic devices.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electronic packaging, and in particular to a nano solder paste, a solder joint and a preparation method thereof. Background Art
[0002] Electronic packaging materials include polymer materials, ceramic materials, metal materials and metal composites. For a long time, metals or metal composites such as Cu, Al, Kovar, tungsten copper, molybdenum copper, aluminum silicon carbide, etc. have been used as heat sinks, carriers, shells and other heat-conducting and heat-dissipating components for high-power electronic devices. However, as the size of devices continues to decrease and the power continues to increase, the requirements for the thermal conductivity of packaging materials are also getting higher and higher. Diamond copper is a metal-based composite material with copper as the matrix and diamond particles as the reinforcement phase. Its thermal conductivity can reach 800W / (m·K), and its thermal expansion coefficient matches that of common Si, GaN, SiC and other materials. It is an ideal heat dissipation packaging material. However, due to the exposed diamond particles on the surface of diamond copper, common metal materials have poor affinity with diamond particles. Therefore, compared with metals or metal composites, welding materials such as AuSn, SnAg, SnAgCu, and sintered silver paste have worse wettability on the surface of diamond copper, and the solder cannot spread and does not react with diamond. If conventional welding materials and packaging processes are used, the connection strength between chips, tube shell walls and other materials and diamond copper is low and the long-term reliability is poor.
[0003] At present, in order to solve the connection problem between diamond copper and chips, the surface of diamond copper often needs to be plated. A nickel layer is formed on the surface of diamond copper by chemical plating, that is, after sensitization and activation treatment with strong reducing ions, a catalytic reduction center of copper ions is formed on the surface of diamond particles, which promotes the deposition of nickel ions and obtains a nickel plating layer with high bonding strength, uniformity and density. Then, the nickel layer is thickened or plated with a layer of metal such as Pd and Au by electroplating. The surface plating of diamond copper improves the solderability of diamond copper, and the solder can be wetted, thereby completing the welding of the chip and diamond copper. However, the sensitization and activation treatment of diamond copper will cause the roughness of the diamond copper surface to increase, affecting the subsequent chip packaging process; the plating layer does not undergo metallurgical bonding with the diamond particles, the bonding force is weak, the thermal expansion coefficient is relatively different, and it is easy to fall off after experiencing high temperature, affecting the reliability of the chip; the thermal conductivity of the plating layer is low, which reduces the overall heat dissipation capacity of the diamond copper material. Summary of the invention
[0004] Based on this, the present invention provides a nano solder paste which can improve the welding bonding strength between diamond copper and chip, and enhance the reliability and heat dissipation capability.
[0005] A nano solder paste, which is composed of 30% to 60% soldering flux, 5% to 10% nano particle dispersant and the remainder of base solder powder in terms of mass percentage; the nano particle dispersant includes 65% to 85% of metal nano particles and the remainder of polymer dispersant, the metal nano particles are metal particles that can undergo metallurgical reaction with diamond, and the particle size of the metal nano particles is 10 to 800 nm; the soldering flux includes resin, activator, organic solvent and thixotropic agent.
[0006] Preferably, the nano solder paste is composed of 40% to 48% of soldering flux, 6% to 8% of nano particle dispersant and the remainder of base solder powder.
[0007] In one embodiment, the metal nanoparticles are selected from one or more of Ti, Mo, Cr, W and Ta nanoparticles.
[0008] In one embodiment, the metal nanoparticles are Ti and / or Ta nanoparticles with a particle size of 50 to 200 nm.
[0009] In one embodiment, the polymer dispersant is selected from one or more of ethyl cellulose, polyvinyl pyrrolidone (PVP), polyethylene glycol, tannic acid and polyvinyl alcohol.
[0010] In one of the embodiments, the soldering flux is composed of 25% to 33% of the resin, 3% to 6% of the activator, 55% to 60% of the organic solvent and the remainder of the thixotropic agent, calculated by mass percentage, and the viscosity of the soldering flux is 120 Pa·s to 200 Pa·s.
[0011] In one embodiment, the resin includes rosin resin, synthetic resin and derivatives thereof, preferably selected from one or more of gum rosin, wood rosin, polyurethane resin, polyester resin, polymerized rosin, hydrogenated rosin and water-white rosin; the active agent is an organic acid, preferably selected from one or more of lactic acid, acrylic acid, benzoic acid, salicylic acid, anisic acid, citric acid and succinic acid; the organic solvent is an alcohol or an ether, preferably selected from one or more of isopropanol, ethylene glycol, glycerol, terpineol, ethylene glycol monomethyl ether and diethylene glycol monoethyl ether; the thixotropic agent is a wax-based thixotropic agent and / or an amide-based thixotropic agent, preferably selected from one or more of hydrogenated castor oil, hydroxystearamide, saturated fatty amide, stearamide, erucamide, unsaturated fatty amide, lauramide and palmitamide.
[0012] In one embodiment, the base solder powder is selected from one or more of AuSn and SnAg (Cu) powders, and has a particle size of 100 to 600 μm, preferably 175 to 360 μm.
[0013] In one of the embodiments, in terms of mass percentage, 15%≤Sn≤75% of the AuSn, 85%≤Sn≤95% of the SnAg(Cu), and 5%≤Ag / (Ag+Cu)≤15%.
[0014] The present invention also provides a method for preparing a welding joint, comprising the following steps: applying the nano solder paste to the diamond copper and / or the area to be welded of the part to be welded, abutting the area to be welded of the diamond copper with the area to be welded of the part to be welded, and then welding to obtain the welding joint.
[0015] In one of the embodiments, welding specifically includes the following steps: placing the diamond copper and the parts to be welded into a reflow furnace, heating them to 200-220°C at a rate of 2-3°C / s, keeping them warm for 80-100s, then continuing to heat them to 350-400°C at the same rate, keeping them warm for 40-60S, and then cooling them to room temperature at a rate of 5-8°C / s.
[0016] The present invention also provides a welding joint, which is prepared according to the above preparation method.
[0017] The above solution of the present invention has the following beneficial effects:
[0018] The present invention provides a nano solder paste that can directly solder parts to diamond copper, a solder joint formed by the two, and a corresponding soldering method. A small amount of nano active metal particles and a polymer dispersant are added to the nano solder paste, which is specially used for the welding of diamond copper. The bonding force between the surface coating of the diamond copper and the diamond particles is not high, and metallization treatment is not required on the diamond particles, so sensitization and activation treatment is not required, the roughness of the diamond copper will not increase, and the heat transfer capacity will also be enhanced; under suitable process conditions, the nano solder paste can directly react metallurgically with the diamond particles on the diamond copper material at a lower temperature to form a more solid solder joint, simplifying the packaging process and further improving the reliability of electronic devices. The solder joint is suitable for connecting electronic packaging chips with diamond copper heat sinks and carriers, and connecting tube shell walls with diamond copper bases, and is widely used. DETAILED DESCRIPTION
[0019] In order to make the technical problems, technical solutions and advantages to be solved by the present invention clearer, the following will be described in detail in conjunction with specific embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0020] In addition, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other. The reagents and instruments used in the examples are conventionally selected in the art unless otherwise specified. The experimental methods without specific conditions in the examples are implemented according to conventional conditions, such as the conditions described in the literature, books or methods recommended by the manufacturer.
[0021] Example 1
[0022] 1. Nano solder paste: According to the mass percentage, the nano solder paste contains 40% flux, 7% Ta nanoparticle dispersant and the remainder of Au80Sn20 solder powder particles with a particle size of 230-360μm. The flux is 32% rosin resin, 58% ethylene glycol solvent, 5.2% lactic acid and the remainder hydrogenated castor oil thixotropic agent; the Ta nanoparticle dispersant is 82% Ta particles with a particle size of 120-230nm and 18% PVP dispersant.
[0023] 2. Welding joint: Use 50W GaN on SiC chip, chip size 12.5*8.6*0.475mm, Ti / Ni / Ag metal layers are deposited on the surface in sequence, diamond copper size 20*10*1mm (surface not metallized). Apply solder paste to the diamond copper surface of the area to be welded, with a thickness of 35μm, put the diamond copper and the chip or shell to be welded into the reflow oven, heat up to 200℃ at a rate of 3℃ / s, keep warm for 85s, continue to heat up to 380℃ at the same rate, keep warm for 45S, and then cool to room temperature at a cooling rate of 8℃ / s.
[0024] Example 2
[0025] 1. Nano solder paste: According to the mass percentage, the nano solder paste contains 48% solder flux, 6% Ti nanoparticle dispersant and the remainder of Au80Sn20 solder powder particles with a particle size of 230-360μm. The solder flux is 32% rosin resin, 58% ethylene glycol solvent, 5.2% lactic acid and the remainder hydrogenated castor oil thixotropic agent; the Ti nanoparticle dispersant is 82% Ti particles with a particle size of 100-200nm and 18% PVP dispersant.
[0026] 2. Welding joint: Use 50W GaN on SiC chip, chip size 12.5*8.6*0.475mm, Ti / Ni / Ag metal layers are deposited on the surface in sequence, diamond copper size 20*10*1mm (surface not metallized). Apply solder paste to the diamond copper surface of the area to be welded, with a thickness of 35μm, put the diamond copper and the chip or shell to be welded into the reflow oven, heat up to 200℃ at a rate of 3℃ / s, keep warm for 85s, continue to heat up to 380℃ at the same rate, keep warm for 45S, and then cool to room temperature at a cooling rate of 8℃ / s.
[0027] Example 3
[0028] The difference between this embodiment and Example 1 is that Ta particles are replaced by Mo particles, and the remaining components and welding process are the same.
[0029] Example 4
[0030] The difference between this embodiment and Example 1 is that Ta particles are replaced by Cr particles, and the remaining components and welding process are the same.
[0031] Example 5
[0032] The difference between this embodiment and Example 1 is that Ta particles are replaced by W particles, and the remaining components and welding process are the same.
[0033] Comparative Example 1
[0034] The difference between this embodiment and Example 1 is that no nanoparticle dispersant is added to the nano solder paste, and the remaining components and welding process are the same.
[0035] Comparative Example 2
[0036] The difference between this embodiment and Example 1 is that the particle size of the metal nanoparticles is 1000-1400 nm, and the other components and welding process are the same.
[0037] Comparative Example 3
[0038] The present embodiment is different from Example 1 in that the surface of the diamond copper is metallized, wherein the nickel layer is 7-10 μm, the gold layer is 1-1.6 μm, and no nanoparticle dispersant is added to the solder paste. The remaining components and welding process are the same.
[0039] Comparative Example 4
[0040] The difference between this embodiment and Example 1 is that the metal nanoparticles are Ni, and the other components and welding process are the same.
[0041] Comparative Example 5
[0042] The present embodiment is different from Example 1 in that the nano solder paste contains 40% of flux, 15% of Ta nanoparticle dispersant and the remainder of Au80Sn20 solder powder particles with a particle size of 230 to 360 μm, and the remaining ingredients and welding process are the same.
[0043] The nano solder pastes prepared in each embodiment and each comparative example were subjected to shear strength and wettability tests and chip shell temperature tests. The test results are shown in Table 1 below.
[0044] The test method is as follows: 1) Shear strength test: Use a shear tester to test the shear strength of the welded joint, with the pusher distance of 0.1mm from the surface of the diamond copper heat sink and the pusher speed of 0.1mm / s. 2) Wettability: Apply each newly produced nano solder paste on the diamond copper plate, with a length and width of 10mm and a thickness of 30 microns. In a nitrogen atmosphere, heat from 25℃ to 400℃ at a heating rate of 2℃ / second, cool to room temperature, and then count the spread area of the nano solder on the diamond copper plate, and calculate the area percentage of the original solder layer; 3) Chip shell temperature: Place the diamond copper with the soldered chip on a liquid-cooled radiator coated with thermal interface material on the surface, keep the temperature of the cooling water in the radiator at 50℃, use an infrared thermal imager to test the temperature of the chip surface, and measure the chip shell temperature.
[0045] Table 1 Performance test results
[0046] Shear strength(MPa) Wettability Chip case temperature (℃) Example 1 113 115.6% 109 Example 2 107 116.3% 107 Example 3 116 118.8% 105 Example 4 111 116.8% 108 Example 5 98 111.5% 112 Comparative Example 1 25 75.2% 138 Comparative Example 2 64 87.6% 116 Comparative Example 3 84 117.2% 118 Comparative Example 4 32 85% 141 Comparative Example 5 59 95% 128
[0047] In comparative example 1, due to the lack of specific metal nanoparticles in the nano solder paste, the solder cannot be wetted and spread, the shear strength is extremely low, there is a considerable interface thermal resistance between the chip and the diamond copper, and the chip junction temperature is high;
[0048] In comparative example 2, since the metal nanoparticles in the nano solder paste have a large particle size and poor reactivity, the temperature required for the metallurgical reaction to occur is too high, so the welding effect is poor when the same welding temperature is used;
[0049] Comparative Example 3 adopts the currently common welding process. Since a metal layer is deposited on the surface of the diamond copper, the thermal resistance is relatively large, the heat dissipation performance is slightly worse, and the shear strength is relatively low.
[0050] In comparative example 4, since the metal nanoparticles Ni used cannot undergo metallurgical reaction with diamond, the solder cannot wet and spread, the shear strength is extremely low, there is a considerable interface thermal resistance between the chip and the diamond copper, and the junction temperature of the chip is relatively high.
[0051] In Comparative Example 5, due to excessive amounts of metal nanoparticles, they cannot form a good synergistic effect with the flux and the base solder powder, resulting in poor welding effect.
[0052] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A nano solder paste, characterized in that: The invention is composed of 30% to 60% soldering flux, 5% to 10% nanoparticle dispersant and the remainder of base solder powder in terms of mass percentage; the nanoparticle dispersant comprises 65% to 85% of metal nanoparticles and the remainder of polymer dispersant, the metal nanoparticles are metal particles that can undergo metallurgical reaction with diamond, and the particle size of the metal nanoparticles is 10 to 800 nm; the soldering flux comprises resin, activator, organic solvent and thixotropic agent.
2. The nano solder paste according to claim 1, characterized in that: The metal nanoparticles are selected from one or more of Ti, Mo, Cr, W and Ta nanoparticles.
3. The nano solder paste according to claim 1, characterized in that: The metal nanoparticles are Ti and / or Ta nanoparticles with a particle size of 50 to 200 nm.
4. The nano solder paste according to claim 1, characterized in that: The polymer dispersant is selected from one or more of ethyl cellulose, polyvinyl pyrrolidone, polyethylene glycol, tannic acid and polyvinyl alcohol.
5. The nano solder paste according to any one of claims 1 to 4, characterized in that: Calculated by mass percentage, the soldering flux consists of 25% to 33% of the resin, 3% to 6% of the activator, 55% to 60% of the organic solvent and the balance of the thixotropic agent.
6. The nano solder paste according to any one of claims 1 to 4, characterized in that: The resin is selected from one or more of gum rosin, wood rosin, polyurethane resin, polyester resin, polymerized rosin, hydrogenated rosin and water-white rosin; the active agent is selected from one or more of lactic acid, acrylic acid, benzoic acid, salicylic acid, anisic acid, citric acid and succinic acid; the organic solvent is selected from one or more of isopropyl alcohol, ethylene glycol, glycerol, terpineol, ethylene glycol monomethyl ether and diethylene glycol monoethyl ether; the thixotropic agent is selected from one or more of hydrogenated castor oil, hydroxystearamide, saturated fatty amide, stearamide, erucamide, unsaturated fatty amide, lauramide and palmitamide.
7. The nano solder paste according to any one of claims 1 to 4, characterized in that: The base solder powder is selected from one or more of AuSn and SnAg (Cu) powders, and has a particle size of 100 to 600 μm.
8. The nano solder paste according to claim 7, characterized in that: In terms of mass percentage, in the AuSn, 15%≤Sn≤75%, in the SnAg(Cu), 85%≤Sn≤95%, and 5%≤Ag / (Ag+Cu)≤15%.
9. A method for preparing a welded joint, characterized in that: The method comprises the following steps: applying the nano solder paste described in any one of claims 1 to 8 to the diamond copper and / or the area to be welded of the part to be welded, abutting the area to be welded of the diamond copper with the area to be welded of the part to be welded, and then welding to obtain the welded joint.
10. A welding joint, characterized in that: Prepared according to the preparation method according to claim 9.