Metal grinding wheel for quartz grinding and preparation method thereof
By using a metal grinding wheel composed of titanium-plated diamond and copper-tin alloy powder, combined with cold prepression and hot pressing sintering processes, the problems of low processing efficiency and high scratch rate of quartz grinding wheels are solved, and higher wear resistance is achieved and lower production costs.
Patent Information
- Application Number
- CN202411215319.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-09-02
AI Technical Summary
The existing quartz grinding wheels have low processing efficiency, easy to collapse, scratch and serious abrasive marks.
The metal grinding wheel consisting of titanium-plated diamond, copper powder, tin powder, molybdenum disulfide, graphite and copper-tin alloy powder were prepared by cold prepression and hot pressing sintering processes. The inclination angle of the grinding teeth is 30° and the sintering temperature is 500. ℃~600°C, pressure between 80Mpa~100Mpa, low melting point copper-tin alloy powder is used as the metal bonding agent.
It improves the wear resistance of the grinding wheel and the thermal damage during electric spark processing, reduces production costs, reduces the thermal damage of diamonds, reduces the scratch rate, and improves the grinding efficiency.
Smart Images

Figure CN118990359A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of grinding wheel preparation, and in particular to a metal grinding wheel for quartz grinding and a preparation method thereof. Background Art
[0002] As an important material in semiconductor technology, quartz material has many excellent properties and wide applications. Its high hardness, high temperature resistance and chemical stability make it an ideal semiconductor material. Through appropriate preparation methods, quartz materials of different shapes and sizes can be obtained to meet different needs. In semiconductor technology, quartz materials are widely used in wafer substrates, photolithography grinding substrates, insulation materials and packaging materials, providing reliable support for semiconductor manufacturing. With the continuous development of semiconductor technology, the application prospects of quartz materials will be broader. It is precisely because quartz has high hardness, strength and wear resistance that the precision quartz grinding process widely used in the semiconductor field has always been low in efficiency, edge collapse, scratches, and serious grinding marks. Summary of the invention
[0003] In view of the above-mentioned shortcomings of the prior art, the purpose of the present invention is to provide a metal grinding wheel for quartz grinding and a preparation method thereof, so as to effectively solve the problems of low processing efficiency, easy edge collapse, scratches, severe grinding marks, etc. of other traditional grinding wheels.
[0004] The present invention first provides a metal grinding wheel for quartz grinding, which comprises a base and grinding teeth arranged on one end surface of the base, a through hole is opened in the middle of the base, and the grinding teeth are composed of the following raw materials in weight percentage: 5% to 15% titanium-plated diamond; 5% to 10% copper powder; 10% to 15% tin powder; 2% to 6% molybdenum disulfide; 3% to 5% graphite; and the balance is copper-tin alloy powder.
[0005] More optimally, the mass fraction of tin in the copper-tin alloy is 30% to 50%. The mass fraction of tin in the copper-tin alloy cannot be too high. If the tin content is too high, overflow will occur during hot pressing, causing component segregation.
[0006] More optimally, the grinding teeth have an inclination angle α of 30° relative to the center line of the base.
[0007] More optimally, the mesh size of the titanium-coated diamond is 325-800 meshes.
[0008] Another aspect of the present invention further provides a method for preparing a metal grinding wheel for quartz grinding, comprising the following steps:
[0009] Mix the raw materials evenly to obtain molding material;
[0010] The molding material is placed into a molding die for cold pre-pressing, and then hot-pressed and sintered to obtain a grinding tooth;
[0011] Compounding an upper substrate on one end of the grinding tooth to obtain the quartz grinding metal grinding wheel;
[0012] The metal grinding wheel comprises a base and grinding teeth arranged on one end surface of the base, a through hole is opened in the middle of the base, and the grinding teeth are composed of the following raw materials in weight percentage: 5% to 15% titanium-plated diamond; 5% to 10% copper powder; 10% to 15% tin powder; 2% to 6% molybdenum disulfide; 3% to 5% graphite; and the balance is copper-tin alloy powder.
[0013] More optimally, the raw material mixing includes wetting the titanium-coated diamond with a wetting agent, and the wetting agent is a mixture of one or more of cresol, polyvinyl alcohol, and liquid paraffin.
[0014] More optimally, during the hot pressing sintering process, the sintering temperature is 500° C. to 600° C., the pressure is 80 MPa to 100 MPa, and the insulation time is 30 min to 40 min.
[0015] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0016] (1) The metal binder of the present invention is mainly composed of copper-tin alloy powder with a low melting point, which reduces the sintering temperature of the metal binder and has a strong diamond holding force. Titanium-coated diamond is used as an abrasive to increase the bonding force between diamond and the binder, improve the wear resistance of the grinding wheel and the thermal damage during electric spark machining.
[0017] (2) The metal bond diamond grinding wheel of the present invention can be sintered at a temperature below 600° C. The sintering temperature is relatively low, which reduces production costs and reduces thermal damage to diamond.
[0018] (3) The oblique grinding teeth have a lower scratch rate and facilitate the timely removal of cooling water during grinding. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 It is a front view of the metal grinding wheel prepared in Example 1 of the present invention;
[0020] Figure 2 is a cross-sectional view of a metal grinding wheel prepared in Example 1 of the present invention;
[0021] Figure 3 This is a schematic diagram of the metal grinding wheel grinding teeth prepared in Example 1 of the present invention;
[0022] Figure 4 Schematic diagram of the cylindrical tooth structure metal grinding wheel in Comparative Example 1;
[0023] Figure 5 The morphology of the cylindrical tooth structure metal grinding wheel in Comparative Example 1 after one week of use is shown. DETAILED DESCRIPTION
[0024] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] like Figure 1 As shown, the metal grinding wheel comprises a base 1 and grinding teeth 2 arranged on one end surface of the base 1, the grinding teeth 2 are evenly distributed on one end surface of the base 1, a through hole 3 is opened in the middle of the base 1, and the grinding teeth 2 are composed of the following raw materials in weight percentage: 5% to 15% titanium-plated diamond; 5% to 10% copper powder; 10% to 15% tin powder; 2% to 6% molybdenum disulfide; 3% to 5% graphite; the remainder is copper-tin alloy powder; wherein the mass fraction of tin in the copper-tin alloy is 30% to 50%, and the mass fraction of tin in the copper-tin alloy cannot be too high. If the tin content is too high, it will overflow during hot pressing, causing component segregation. The number of the grinding teeth 2 is 120, the diameter R of the metal grinding wheel is 560mm, and the diameter Y of the through hole 3 is 350mm. The inclination angle α of the grinding teeth 2 relative to the center line of the base 1 is 30°. The height D of the grinding teeth 2 is 10 mm, and the structure of the grinding teeth 2 may be a racetrack-shaped structure. The length L of the racetrack-shaped structure is 15 mm, the width W is 5 mm, and the radius Q of the arc is 2.5 mm.
[0026] The titanium-coated diamond was purchased from Sandvik, model MBG680Ti.
[0027] Embodiment 1:
[0028] Step 1: Mix the raw materials 325 mesh 10% titanium-coated diamond, 8% copper powder, 12% tin powder, 4% molybdenum disulfide, 3% graphite, and 63% copper-tin alloy powder Cu67Sn33 evenly and put them into a molding mold for cold pre-pressing, wherein the mixing includes first mixing the copper powder, tin powder, molybdenum disulfide, and copper-tin alloy powder Cu67Sn33 through a 400-mesh sieve and then adding the titanium-coated diamond for mixing, and adding paraffin at a ratio of 1 drop of paraffin per 100g of raw material and continuing to mix, and after mixing for 1 hour, pass through a 150-mesh sieve, the cold pre-pressing pressure is 30Mpa, and the cold pre-pressing time is 10s.
[0029] Step 2: The cold pre-pressed molding material and the mold in step 1 are put into a bell-shaped furnace with hydrogen and nitrogen protective gas for hot pressing and sintering. The hot pressing and sintering time includes heating time and holding time. The hot pressing and sintering time is 3 hours, of which the holding time is 30 minutes, the pressure is 80 MPa, and the hot pressing and sintering temperature is 500°C. After the hot pressing and sintering is completed, the hot pressing and sintering molding material is demolded to obtain the grinding wheel grinding teeth.
[0030] Step 3: The grinding teeth obtained in step 2 are bonded to the substrate, and the semi-finished product is turned and ground to form a metal grinding wheel for quartz grinding. The number of the grinding teeth 2 is 120, the diameter R of the metal grinding wheel is 560 mm, the diameter Y of the through hole 3 is 350 mm, and the inclination angle α of the grinding teeth 2 relative to the center line of the substrate 1 is 30°.
[0031] Embodiment 2:
[0032] Step 1: Mix the raw materials 800 mesh 5% titanium-coated diamond, 10% copper powder, 12% tin powder, 3% molybdenum disulfide, 5% graphite, and 65% copper-tin alloy powder Cu67Sn33 evenly and put them into a molding mold for cold pre-pressing, wherein the mixing includes first mixing the copper powder, tin powder, molybdenum disulfide, and copper-tin alloy powder Cu67Sn33 through a 400 mesh sieve and then adding the titanium-coated diamond for mixing, and adding paraffin at a ratio of 1 drop of paraffin per 100g of raw material and continuing to mix, mixing for 1 hour and passing through a 150 mesh sieve, the cold pre-pressing pressure is 30Mpa, and the cold pre-pressing time is 15s.
[0033] Step 2: The cold pre-pressed molding material and the mold in step 1 are put into a bell-shaped furnace with hydrogen and nitrogen protective gas for hot pressing and sintering. The hot pressing and sintering time includes heating time and holding time. The hot pressing and sintering time is 3 hours, of which the holding time is 35 minutes, the pressure is 80 MPa, and the hot pressing and sintering temperature is 500°C. After the hot pressing and sintering is completed, the hot pressing and sintering molding material is demolded to obtain the grinding wheel grinding teeth.
[0034] Step 3: The grinding teeth obtained in step 2 are bonded to the substrate, and the semi-finished product is turned and ground to form a metal grinding wheel for quartz grinding.
[0035] Embodiment 3:
[0036] Step 1: Mix the raw materials 400 mesh 5% titanium-coated diamond, 10% copper powder, 10% tin powder, 6% molybdenum disulfide, 4% graphite, and 55% copper-tin alloy powder Cu60Sn40 evenly and put them into a molding mold for cold pre-pressing, wherein the mixing includes first mixing the copper powder, tin powder, molybdenum disulfide, and copper-tin alloy powder Cu60Sn40 through a 400 mesh sieve and then adding the titanium-coated diamond for mixing, and adding paraffin at a ratio of 1 drop of paraffin per 100g of raw material and continuing to mix, mixing for 1 hour and passing through a 150 mesh sieve, the cold pre-pressing pressure is 40Mpa, and the cold pre-pressing time is 15s.
[0037] Step 2: The cold pre-pressed molding material and the mold of step 1 are put into a bell-shaped furnace with hydrogen and nitrogen protective gas for hot pressing and sintering. The hot pressing and sintering time includes heating time and holding time. The hot pressing and sintering time is 3 hours, of which the holding time is 35 minutes, the pressure is 80 MPa, and the hot pressing and sintering temperature is 550°C. After the hot pressing and sintering is completed, the hot pressing and sintering molding material is demolded to obtain the grinding wheel grinding teeth.
[0038] Step 3: The grinding teeth obtained in step 2 are bonded to the substrate, and the semi-finished product is turned and ground to form a metal grinding wheel for quartz grinding.
[0039] Implementation 4:
[0040] Step 1: Mix the raw materials 500 mesh 15% titanium-coated diamond, 10% copper powder, 15% tin powder, 6% molybdenum disulfide, 3% graphite, and 51% copper-tin alloy powder Cu60Sn40 evenly and put them into a molding mold for cold pre-pressing, wherein the mixing includes first mixing the copper powder, tin powder, molybdenum disulfide, and copper-tin alloy powder Cu60Sn40 through a 400 mesh sieve and then adding the titanium-coated diamond for mixing, and adding paraffin at a ratio of 1 drop of paraffin per 100g of raw material and continuing to mix, mixing for 1 hour and passing through a 150 mesh sieve, the cold pre-pressing pressure is 40Mpa, and the cold pre-pressing time is 20s.
[0041] Step 2: The cold pre-pressed molding material and the mold in step 1 are put into a bell-shaped furnace with hydrogen and nitrogen protective gas for hot pressing and sintering. The hot pressing and sintering time includes heating time and holding time. The hot pressing and sintering time is 3 hours, of which the holding time is 40 minutes, the pressure is 80 MPa, and the hot pressing and sintering temperature is 550°C. After the hot pressing and sintering is completed, the hot pressing and sintering molding material is demolded to obtain the grinding wheel grinding teeth.
[0042] Step 3, the grinding teeth obtained in step 2 are bonded to the substrate, and the semi-finished product is turned and ground to form a metal grinding wheel for quartz grinding.
[0043] Implementation 5:
[0044] Step 1: Mix the raw materials 400 mesh 15% titanium-coated diamond, 5% copper powder, 10% tin powder, 2% molybdenum disulfide, 5% graphite, and 73% copper-tin alloy powder Cu60Sn40 evenly and put them into a molding mold for cold pre-pressing, wherein the mixing includes first mixing the copper powder, tin powder, molybdenum disulfide, and copper-tin alloy powder Cu60Sn40 through a 400 mesh sieve and then adding the titanium-coated diamond for mixing, and adding paraffin at a ratio of 1 drop of paraffin per 100g of raw material and continuing to mix, and after mixing for 1 hour, pass through a 150 mesh sieve, the cold pre-pressing pressure is 50Mpa, and the cold pre-pressing time is 20s.
[0045] Step 2: The cold pre-pressed molding material and the mold in step 1 are put into a bell-shaped furnace with hydrogen and nitrogen protective gas for hot pressing and sintering. The hot pressing and sintering time includes heating time and holding time. The hot pressing and sintering time is 3 hours, of which the holding time is 40 minutes, the pressure is 80 MPa, and the hot pressing and sintering temperature is 600°C. After the hot pressing and sintering is completed, the hot pressing and sintering molding material is demolded to obtain the grinding wheel grinding teeth.
[0046] Step 3: The grinding teeth obtained in step 2 are bonded to the substrate, and the semi-finished product is turned and ground to form a metal grinding wheel for quartz grinding.
[0047] The grinding wheels obtained in the above embodiments have the same structural parameters, but use different raw materials and processes.
[0048] Comparative Example 1:
[0049] The grinding wheel structure of this comparative example is as follows Figure 4 The preparation method of this comparative example refers to Example 3, except that:
[0050] In Comparative Example 1, the grinding teeth are cylindrical with a diameter of 16 mm and a cross groove with a width of 2 mm and a depth of 5 mm in the middle. There are 67 grinding teeth evenly distributed on the metal grinding wheel, and the height of the grinding teeth is also equal to 10 mm.
[0051] Comparative Example 2:
[0052] The formula of the metal grinding wheel for quartz grinding provided in this comparative example is that the diamond is bare diamond, and the proportions of the other components and the preparation process are the same as those in Example 3.
[0053] Comparative Example 3:
[0054] The metal grinding wheel formula for quartz grinding provided in this comparative example includes, by mass fraction, 400 mesh 5% titanium-coated diamond, 42.4% copper powder, 31.6% tin powder, 6% molybdenum disulfide, 5% graphite, and a hot pressing sintering temperature of 700°C. The preparation method of this comparative example refers to Example 3.
[0055] evaluate:
[0056] The finished grinding wheels prepared in Examples 1 to 5 and Comparative Examples 1 to 3 were subjected to grinding tests on a Shanghai Rijin NVG-1000D equipment.
[0057] Cutting force test method: The cutting force can be determined based on the current value of the cutting equipment load. The smaller the current value, the better the cutting force, and the larger the current value, the worse the cutting force.
[0058] Testing method for scratch rate: visually inspect the scratches on the quartz surface. The scratch rate is the number of pieces with scratches on the surface after grinding / the total number of processed pieces.
[0059] Stability test: Observe the appearance of the grinding teeth after one week of use.
[0060] The effects of each embodiment and comparative example are shown in the following table.
[0061] Table 1 Comparison of the use effects of various embodiments and comparative examples
[0062]
[0063] Conclusion: Example 3 has the lowest scratch rate. 400 mesh diamond has better surface roughness than coarser diamond, and finer diamond has better cutting force. Example 2 has a high graphite content, and there is a tendency for the scratch rate to increase and the cutting force to weaken. The cylindrical grinding teeth set in Comparative Example 1 will cause cooling water to accumulate on the cylindrical teeth; Comparative Example 2 uses diamonds that are not titanium-plated, which has a higher scratch rate on quartz. The sintering temperature of Comparative Example 3 needs to reach 700°C, which has a higher scratch rate on quartz. In addition, Figure 5 As shown, after a certain period of use, the cylindrical grinding tooth edge in Comparative Example 1 has the risk of easy chipping.
[0064] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0065] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A metal grinding wheel for quartz grinding, characterized in that: The metal grinding wheel comprises a base and a grinding tooth arranged on one end surface of the base, a through hole is opened in the middle of the base, and the grinding tooth is composed of the following raw materials in weight percentage: 5% to 15% titanium-coated diamond; 5% to 10% copper powder; 10%~15% tin powder; 2% to 6% molybdenum disulfide; 3% to 5% graphite; The balance is copper-tin alloy powder.
2. A metal grinding wheel for quartz grinding according to claim 1, characterized in that: The mass fraction of tin in the copper-tin alloy is 30% to 50%.
3. A metal grinding wheel for quartz grinding according to claim 1, characterized in that: The grinding teeth have an inclination angle α of 30° relative to the center line of the base body.
4. The metal grinding wheel for quartz grinding according to claim 1, characterized in that: The mesh number of the titanium-coated diamond is 325-800 meshes.
5. A method for preparing a metal grinding wheel for quartz grinding, characterized in that: The following steps are involved: Mix the raw materials evenly to obtain molding material; The molding material is placed in a molding die for cold pre-pressing, and then hot-pressed and sintered to obtain a grinding tooth; Compounding an upper substrate on one end of the grinding tooth to obtain the quartz grinding metal grinding wheel; The metal grinding wheel comprises a base and grinding teeth arranged on one end surface of the base, a through hole is opened in the middle of the base, and the grinding teeth are composed of the following raw materials in the following weight percentages: 5% to 15% titanium-coated diamond; 5% to 10% copper powder; 10%~15% tin powder; 2% to 6% molybdenum disulfide; 3% to 5% graphite; The balance is copper-tin alloy powder.
6. The preparation method according to claim 5, characterized in that: The raw material mixing includes wetting the titanium-coated diamond with a wetting agent, wherein the wetting agent is one or a mixture of cresol, polyvinyl alcohol, and liquid paraffin.
7. The preparation method according to claim 5, characterized in that: In the hot pressing sintering process, the sintering temperature is 500° C. to 600° C., the pressure is 80 MPa to 100 MPa, and the heat preservation time is 30 min to 40 min.
Citation Information
Patent Citations
Grinding device and grinding method thereof
CN107009262A
Metal bonding agent, metal bonding agent diamond grinding wheel and preparing method of metal bonding agent diamond grinding wheel
CN108972374A
Prealloy powder used by compound binding agent grinding tool for grinding hard and brittle material, preparation method of prealloy powder and grinding tool
CN110508800A
Diamond grinding wheel and preparation process thereof
CN116890308A
Grinding wheel for grinding edges of glass substrates and method of manufacturing of the same
EP2671677A2