Ultrahigh molecular weight polyethylene resin sheet, preparation and application thereof, and coiled material
By adopting tensile rheology technology and special mold design in the biaxial eccentric rotor extrusion plasticization subsystem, the processing problem of ultra-high molecular weight polyethylene resin is solved, ensuring the maintenance of its viscosity average molecular weight and performance, and achieving efficient preparation High temperature resistant and puncture-resistant waterproof coil material.
Patent Information
- Application Number
- CN202411122358.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-22
AI Technical Summary
The prior art is difficult to effectively process ultra-high molecular weight polyethylene resin, resulting in breakage of its molecular chain, degradation of viscosity average molecular weight and degradation of performance, and it is difficult to prepare waterproof coils with high wear and impact resistance.
The biaxial eccentric rotor extrusion plasticization subsystem is designed using tensile rheology technology. The rotor combination section with gradually reduced pitch and the straight extrusion reinforcement section can be avoided by avoiding molecular chain breakage. Combined with the special sheet mold design, it ensures stickiness. The retention rate of average molecular weight shall not be less than 80%.
It realizes efficient processing of ultra-high molecular weight polyethylene resin sheets, maintains its high wear and impact resistance, broadens the processing temperature range, and prepares high temperature resistance, puncture resistance, flexible waterproof coils suitable for building waterproofing application.
Smart Images

Figure CN118990973A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of polymer waterproofing coiled materials, and more specifically, relates to an ultra-high molecular weight polyethylene resin sheet, preparation and application thereof, and a coiled material. Background Art
[0002] At present, polymer waterproofing membranes are mainly made of PVC, EPDM, TPO, and HDPE, and are used in underground waterproofing projects and roof waterproofing. Among them, high-density polyethylene is one of the most commonly used materials, usually using a single-screw extrusion process. The viscosity-average molecular weight of polyethylene resin used for waterproofing boards is less than 1 million, the melt mass flow rate is generally higher than 0.1g / 10min, and the melting point is lower than 135℃.
[0003] Ultra-high molecular weight polyethylene with a viscosity-average molecular weight higher than 1 million has excellent physical properties because the molecular chains are easily entangled:
[0004] (1) High wear resistance and self-lubrication: Ultra-high molecular weight polyethylene has self-lubrication second only to polytetrafluoroethylene and has a very small friction coefficient. Its wear resistance is the best among all engineering plastics currently, and its wear resistance is 10 times that of PVC-U and HDPE.
[0005] (2) Low temperature resistance, impact resistance, and corrosion resistance: Ultra-high molecular weight polyethylene still has high impact resistance at low temperatures, and is particularly suitable for applications in cold regions. For ultra-high molecular weight polyethylene pipes, the service life under strong corrosion and high wear conditions is 4-6 times that of steel pipes.
[0006] Ultra-high molecular weight polyethylene has the characteristics of being difficult to process due to its ultra-long molecular chain structure and high entanglement density. The melt mass flow rate is 0, and it also behaves as a high-viscosity elastic body when heated to the melting temperature. The relationship between melt viscosity and viscosity-average molecular weight can be expressed by the following formula, where k is a constant and M is wc is the critical viscosity-average molecular weight. When the viscosity-average molecular weight is higher than the critical viscosity-average molecular weight, the physical crosslinking formed by the entanglement of the molecular chains increases the melt viscosity. Generally, the viscosity-average molecular weight of polymers is much greater than M wc , from the formula, we can get that the viscosity-average molecular weight is 10 times higher and the viscosity is two thousand times higher.
[0007] η=kM w (M w <M wc );
[0008] η=kM w 3.4 (M w >M wc );
[0009] It is difficult to process using a single or twin screw extruder that normally processes ordinary HDPE. At the same time, it is easy to slip on the screw wall because of its small friction coefficient. It is highly elastic between the melting point and the decomposition temperature. If the heating time is too long, the material will be oxidized and degraded.
[0010] Using the traditional screw processing method based on shear rheological field, medium and low viscosity average molecular weight HDPE, LDPE, LLDPE and ultra-high molecular weight polyethylene can be blended and modified, or other processing aids can be added to improve melt fluidity for extrusion processing. A counter-rotating screw can also be used to force the melt to be transported, but due to excessive shear force, the molecular weight of the extruded material decreases by about 40%, and the performance is greatly reduced. There are also documents proposing the use of a grinding disc-shaped mechanochemical reactor with strong shear force for processing, but it will lead to a serious decrease in molecular weight, making the molecular weight of the product far lower than the original molecular weight of the ultra-high molecular weight resin, so that the product does not have the high strength and impact resistance physical properties that ultra-high molecular weight polyethylene should have. The processing of ultra-high molecular weight polyethylene also includes compression molding, plunger extrusion, injection molding, and blow molding. The high shear force generated by the above-mentioned processing equipment will cause the molecular chain to break, and on the other hand, the long thermal mechanical process will cause the material to thermally decompose.
[0011] Table 1 Performance data of high density polyethylene with different viscosity average molecular weight
[0012]
[0013] Therefore, it is urgent to propose a sheet material and a preparation method of an ultra-high molecular weight polyethylene resin. Summary of the invention
[0014] The purpose of the present invention is to provide an ultra-high molecular weight polyethylene resin sheet, preparation and application, and coiled material in view of the deficiencies of the prior art. The present invention adopts the extensional rheology technology and specially designs the double-axis eccentric rotor extrusion plasticizing subsystem to avoid molecular chain breakage and make the viscosity average molecular weight retention rate of the ultra-high molecular weight polyethylene resin sheet high.
[0015] In order to achieve the above-mentioned object, the first aspect of the present invention provides an ultra-high molecular weight polyethylene resin sheet, wherein the raw material of the sheet comprises an ultra-high molecular weight polyethylene resin having a viscosity average molecular weight of 800,000 to 9,000,000;
[0016] The viscosity average molecular weight of the sheet is not less than 80% of the viscosity average molecular weight of the ultra-high molecular weight polyethylene resin.
[0017] According to the present invention, preferably, the thickness of the sheet is 0.1-2.0 mm.
[0018] According to the present invention, preferably, the raw materials of the sheet include ultra-high molecular weight polyethylene resin with a viscosity-average molecular weight of 800,000 to 9 million, other polymer resins, processing aids and pigments and fillers; and based on the total weight of the sheet, the content of the ultra-high molecular weight polyethylene resin with a viscosity-average molecular weight of 800,000 to 9 million is 55-100%, and the total content of other polymer resins, processing aids and pigments and fillers is 0-45%.
[0019] In the present invention, the processing aid is a processing aid that improves lubrication performance and improves the surface quality of the calendered sheet.
[0020] According to the present invention, preferably, the sheet is made by an extrusion plasticizing system, which includes a barrel, a double-shaft eccentric rotor extrusion plasticizing subsystem, a sheet forming die, a three-roll calendering device and a sheet winding device;
[0021] The double-shaft eccentric rotor extrusion plasticizing subsystem comprises two mutually meshing eccentric rotors and a stator, wherein the eccentric rotor comprises a plurality of eccentric spiral structures and eccentric cylindrical structures, including a feed section, a melt plasticizing section and a melt conveying section sequentially connected from a feed end to a discharge end;
[0022] The feed section comprises a non-eccentric threaded rotor;
[0023] The melt plasticizing section comprises a first rotor assembly section, a straight extrusion reinforcement section and a reflux section which are connected in sequence and gradually decrease in pitch;
[0024] The melt conveying section comprises a melt conveying section 1, a melt conveying section 2 and a second rotor assembly section with a gradually decreasing pitch which are connected in sequence;
[0025] The spiral direction of the reflux section is opposite to that of the other sections of the eccentric rotor.
[0026] In the present invention, as a preferred embodiment, the eccentric rotor contains pins.
[0027] According to the present invention, preferably, the diameter of the eccentric rotor is 20-120 mm, the compression ratio is 2-2.8:1, and the aspect ratio is 38-45:1. (The compression ratio is the ratio of the volume of the first screw groove in the feeding section to the volume of the last screw groove in the melt conveying section.)
[0028] According to the present invention, preferably, the melt plasticizing section and the melt conveying section are multiple sections, and the number of sections, lengths and rotor combination aspect ratio are determined according to the viscosity average molecular weight of the ultra-high molecular weight polyethylene resin. In the present invention, each melt plasticizing section is connected by a third connecting section.
[0029] In the present invention, as a preferred embodiment, Figure 1 As shown:
[0030] The feeding section comprises a pre-feeding section, a first connecting section, a non-eccentric threaded rotor and a second connecting section which are connected in sequence;
[0031] According to one embodiment of the present invention, the length of the pre-feed section is 22-26 mm, and the pitch is 6-10 mm.
[0032] According to one embodiment of the present invention, the lengths of the first connecting segment and the second connecting segment are independently 8-12 mm.
[0033] According to one embodiment of the present invention, there are a plurality of non-eccentric threaded rotors, each of which has a length of 30-120 mm and a pitch of 20-60 mm.
[0034] According to one embodiment of the present invention, the first rotor combination segment with gradually decreasing pitch and the second rotor combination segment with gradually decreasing pitch are each independently a combination segment consisting of at least four pitch segments of a first pitch segment, a second pitch segment, a third pitch segment, a fourth pitch segment and a fifth pitch segment, and each pitch segment has a plurality of pitch segments;
[0035] The first pitch segment has a length of 34-38mm and a pitch of 34-38mm;
[0036] The second pitch segment has a length of 30-33 mm and a pitch of 30-33 mm;
[0037] The third pitch segment has a length of 22-25 mm and a pitch of 22-25 mm;
[0038] The fourth pitch segment has a length of 36-42 mm and a pitch of 18-21 mm;
[0039] The fifth pitch segment has a length of 28-32 mm and a pitch of 12-17 mm;
[0040] According to one embodiment of the present invention, the length of the third connecting segment is 22-26 mm, and the pitch is 6-10 mm.
[0041] According to one embodiment of the present invention, the lengths of the first melt conveying section and the second melt conveying section are each independently 22-26 mm, and the pitches are each independently 6-10 mm.
[0042] According to one embodiment of the present invention, the length of the reflux section is 20-100 mm, the pitch is 3-60 mm, the rotation direction is opposite to the eccentric rotor, and the depth of the screw groove between each screw fin is 1-50 mm.
[0043] According to the present invention, preferably, there are multiple straight extrusion reinforcement sections, each of which has a length of 20-120 mm, a pitch of 5-60 mm, and a screw groove depth of 2-5 mm between each screw fin.
[0044] In a specific embodiment of the present invention, the structure of each eccentric rotor is as follows Figure 1 And as shown in Table 2.
[0045] The pre-feed section corresponds to T45-24-Q8-0A;
[0046] The first connection section and the second connection section both correspond to T45-G10DP-0A;
[0047] The non-eccentric threaded rotor corresponds to 4 T45-40-D40-0A;
[0048] The first rotor combination section with gradually decreasing pitch of the first melting and plasticizing section corresponds to a combination section composed of five pitch sections, namely T45-36-P36-0A, T45-32-P32-0A, T45-24-P24-0A, T45-40-P20-0A and T45-30-P15-0A, and there are 3 T45-36-P36-0A, 2 T45-32-P32-0A, 1 T45-24-P24-0A, 4 T45-40-P20-0A and 3 T45-30-P15-0A.
[0049] The straight extrusion reinforcement section corresponds to 3 T45-30-KP180-3-0A;
[0050] The reflux section corresponds to one T45-30-KP180-3-0B.
[0051] The third connection segment corresponds to T45-24-P8-0A;
[0052] The melt conveying section 1 and the melt conveying section 2 both correspond to T45-24-P8-0A;
[0053] Table 2
[0054]
[0055] According to the present invention, preferably, the die lip of the sheet forming die is a flat-mouth structured film lip, and the thickness of the flat-mouth structured die lip perpendicular to the sheet extrusion direction is 2-20 cm.
[0056] According to the present invention, preferably, an electric heating source and a plurality of temperature sensors are provided on the sheet forming mold, and the plurality of temperature sensors are arranged in a direction parallel to the die lip, and the electric heating source and the plurality of temperature sensors are connected to realize zoned heating in the flow channel of the sheet forming mold.
[0057] In one embodiment of the present invention, Figure 5 As shown, through the electric heating heat source and the multiple temperature sensors, multiple areas are obtained, each area has a temperature sensor socket, so that the temperature setting of area 5-1 and area 5-5 is higher than that of the central area 5-3, and the temperature of the sub-central area 5-2 and the sub-central area 5-4 is between the middle, and the mold has the function of zone heating, which further solves the problem that the UHMW-PE melt affects the fluidity in the flow channel due to uneven temperature. As a preferred solution, the temperature of area 5-1 and area 5-5 is 180°C, the temperature of the sub-central area 5-2 and the sub-central area 5-4 is 170°C, and the temperature of the central area 5-3 is 160°C.
[0058] According to the present invention, preferably, the distance between the die opening of the sheet forming die and the three-roll calendering device is 5-300 mm.
[0059] According to the present invention, preferably, the preparation method of the sheet comprises: feeding the raw material of the sheet from the feeding section into the double-axis eccentric rotor extrusion plasticizing subsystem, after extrusion plasticizing in the first rotor combination section with gradually decreasing pitch and the straight extrusion reinforcement section, the reflux of the material is generated by the reflux section to enhance the extrusion plasticizing and compaction; finally, after achieving uniformity of melt temperature, pressure and degree of plasticization in the melt conveying section, the raw material is fed into the sheet forming mold; the melt coming out of the die lip of the sheet forming mold is subjected to three-roll calendering and winding processing to obtain the sheet.
[0060] In the present invention, the present invention overcomes the processing difficulty of poor fluidity of ultra-high molecular weight polyethylene resin through extrusion plasticization and molding die design, improves the problems of high processing temperature and long thermal shear history of traditional processing methods, broadens the processing temperature range, can be extruded under the condition of less than 240° C., the melt does not sag obviously when it exits the die, has stiffness, and the viscosity average molecular weight retention rate of the ultra-high molecular weight polyethylene resin sheet is not less than 80%, that is, the viscosity average molecular weight of the sheet is not less than 80% of the viscosity average molecular weight of the ultra-high molecular weight polyethylene resin. Specifically:
[0061] (1) In the present invention, the principle of the double-shaft eccentric rotor extrusion plasticizing subsystem to realize the extensional rheology technology is as follows:
[0062] Feeding section: Adopt non-eccentric threaded section with large shear force to realize rapid feeding of raw materials.
[0063] The first melting and plasticizing section: includes a first rotor combination section with a gradually decreasing pitch, and then connected to a straight extrusion reinforcement section. The straight screw ridges contained in the straight extrusion reinforcement section can enhance the extrusion of the material, improve the plasticization, and help the UHMW-PE (ultra-high molecular weight polyethylene) resin to unwind. The reflux section is opposite to the spiral direction of the rotors of the other sections of the eccentric rotor, which helps the material to reflux and compact the material, and further enhances the plasticization and unwinding of the UHMW-PE in the extrusion section.
[0064] The second melt-plasticization section and the third melt-plasticization section: repeat the process similar to the first melt-plasticization section, including a rotor combination with a gradually decreasing pitch, and then connect a straight extrusion reinforcement section. The screw ridges contained in the straight extrusion reinforcement section can further achieve the plasticization and unwinding of UHMW-PE. Generally speaking, the higher the viscosity-average molecular weight of UHMW-PE, the more melt-plasticization sections should be, and the longer the length of the eccentric rotor combination should be.
[0065] Melt conveying section: After the plasticization process of three melting and plasticizing sections, the melt temperature, pressure and plasticization degree are not uniform enough. In order to ensure the uniformity of the final molding material, the material needs to be further processed in the melt conveying section. The melt conveying section is the second rotor combination section with a gradually decreasing pitch, and the last stage of entering the sheet forming mold, which can help the material maintain a compacted state before entering the sheet forming mold.
[0066] The double-axis eccentric rotor extrusion plasticizing subsystem of the present invention allows the ultra-high molecular weight polyethylene resin to be fully plasticized without being subjected to high shear force and a long thermal history time, and the viscosity-average molecular weight of the extruded sheet does not decrease significantly with the increase of the main engine speed, ensuring that the viscosity-average molecular weight retention rate of the sheet is not less than 80%, that is, the viscosity-average molecular weight of the sheet is not less than 80% of the viscosity-average molecular weight of the ultra-high molecular weight polyethylene resin.
[0067] (2) At the same time, the present invention also has a special design for the die lip of the sheet forming die, specifically:
[0068] The die lip of the sheet forming die of the existing common high-density polyethylene extrusion system is shown in Figure 2 The die lip is designed as a pointed mouth type. When the die lip is ejected, the die lip is squeezed and deformed due to the expansion of the ultra-high molecular weight polyethylene melt, making it difficult to ensure uniform transverse thickness.
[0069] Therefore, the present invention can design the die lip into a flat shape (i.e., a flat structure). Figure 3The thickness of the metal material perpendicular to the sheet extrusion direction at the die lip is large, so it has high strength and is not easily deformed by extrusion. The vertical pressure of the melt is not enough to cause the die lip to deform. Because the melt strength of ultra-high molecular weight polyethylene is high, the melt (UHMW-PE) still has strength and stiffness after exiting the die lip (as shown in Figure 6 (a)), so the die lip generally does not need to be directly attached to the surface of the pressure roller. After exiting the die lip, the melt is rolled by the pressure roller to make the sheet thickness uniform and improve the surface flatness. Generally, the ultra-high molecular weight melt has poor fluidity and high strength. The calendering roller should not be too cold. Maintaining a certain temperature can help the ultra-high molecular weight polyethylene sheet to be calendered.
[0070] According to the present invention, preferably, the temperature of each section of the eccentric rotor of the dual-shaft eccentric rotor extrusion plasticizing subsystem is set to be lower than 240°C, preferably 160-220°C.
[0071] According to the present invention, preferably, the extrusion rate of the double-shaft eccentric rotor extrusion plasticizing subsystem is 0.2-12 kg / min. In the present invention, the extrusion rate of the double-shaft eccentric rotor extrusion plasticizing subsystem is not highly correlated with the viscosity average molecular weight of the ultra-high molecular weight polyethylene resin.
[0072] According to the present invention, preferably, the rotation speed of the eccentric rotor of the dual-shaft eccentric rotor extrusion plasticizing subsystem is 5-300 rpm.
[0073] According to the present invention, preferably, the temperature of the three-roll calendering device is 20-200°C, preferably 70°C-150°C.
[0074] The second aspect of the present invention provides a method for preparing the ultra-high molecular weight polyethylene resin sheet, which is carried out in the extrusion plasticizing and molding system, including: feeding the raw material of the sheet from the feeding section into the double-axis eccentric rotor extrusion plasticizing subsystem, after extrusion plasticizing in the first rotor combination section with gradually decreasing pitch and the straight extrusion reinforcement section, the reflux section generates material to strengthen extrusion plasticizing and compaction; finally, after achieving uniformity of melt temperature, pressure and plasticizing degree through the melt conveying section, the raw material is fed into the sheet molding die; the melt coming out of the die lip of the sheet molding die is subjected to three-roll calendering and winding treatment to obtain the sheet.
[0075] The third aspect of the present invention provides the use of the ultra-high molecular weight polyethylene resin sheet in waterproofing rolls. The waterproofing rolls prepared from the ultra-high molecular weight polyethylene resin sheet generally have high temperature resistance (can withstand 90°C high temperature for a long time), high wear resistance, high strength, and high puncture resistance.
[0076] A fourth aspect of the present invention provides a waterproof roll material, comprising an ultra-high molecular weight polyethylene resin sheet and a functional layer disposed on the upper surface of the ultra-high molecular weight polyethylene resin sheet;
[0077] The ultra-high molecular weight polyethylene resin sheet is the ultra-high molecular weight polyethylene resin sheet mentioned above;
[0078] The functional layer includes a hot melt adhesive layer and a weather-resistant anti-stick coating; the ultra-high molecular weight polyethylene resin sheet, the hot melt adhesive layer and the weather-resistant anti-stick coating are arranged in sequence from top to bottom; or, the functional layer is at least one of a PVDF film, a PVF film and a weather-resistant metal foil coated with a weather-resistant coating; or, the functional layer is an upper self-adhesive layer;
[0079] Optionally, the lower surface of the ultra-high molecular weight polyethylene resin sheet is provided with a lower self-adhesive layer;
[0080] Preferably, the thickness of the hot melt adhesive layer is 0.2-1.5 mm;
[0081] Preferably, the thickness of the upper self-adhesive layer and the lower self-adhesive layer is independently 0.2-1.5 mm.
[0082] As a preferred solution, the waterproofing membrane is a pre-laid reverse-adhesive ultra-high molecular weight waterproofing membrane, which includes an ultra-high molecular weight polyethylene resin sheet, a hot melt adhesive layer and a weather-resistant anti-adhesive coating arranged in sequence from top to bottom. The pre-laid reverse-adhesive ultra-high molecular weight waterproofing membrane has high wear resistance and puncture resistance, and can meet the construction requirements without a protective layer after construction.
[0083] As a preferred solution, the waterproofing membrane is a pre-laid reverse-adhesive ultra-high molecular weight waterproofing membrane, which includes a lower self-adhesive layer, an ultra-high molecular weight polyethylene resin sheet, a hot melt adhesive layer and a weather-resistant anti-adhesive coating arranged in sequence from top to bottom. The pre-laid reverse-adhesive ultra-high molecular weight waterproofing membrane has high wear resistance and puncture resistance, and can meet the construction requirements without a protective layer after construction.
[0084] As a preferred embodiment, the waterproof membrane is an exposed self-adhesive ultra-high molecular weight polyethylene waterproof membrane, and the exposed self-adhesive ultra-high molecular weight polyethylene waterproof membrane includes a lower self-adhesive layer, an ultra-high molecular weight polyethylene resin sheet and an exposed functional layer arranged in sequence from top to bottom, and the exposed functional layer is at least one of a PVDF film, a PVF film and a weather-resistant metal foil coated with a weather-resistant coating. Preferably, the weather-resistant metal foil coated with a weather-resistant coating is a weather-resistant aluminum foil.
[0085] As a preferred solution, the waterproof roll is a self-adhesive waterproof roll, which includes an ultra-high molecular weight polyethylene resin sheet and an upper self-adhesive layer arranged in sequence from top to bottom. The self-adhesive waterproof roll has high wear resistance and puncture resistance, and can meet construction requirements without a protective layer after construction.
[0086] The beneficial effects of the technical solution of the present invention are as follows:
[0087] The present invention adopts the stretching rheology technology and specially designs the double-axis eccentric rotor extrusion plasticizing subsystem (eccentric rotor), which can avoid molecular chain breakage and make the viscosity average molecular weight retention rate of ultra-high molecular weight polyethylene resin sheet high. At the same time, the processing technology is energy-saving and efficient. The processing conditions adopt the barrel temperature equivalent to the current high-density polyethylene sheet processing, and the extrusion efficiency is equivalent to the processing of high-density polyethylene sheets, so that a flexible waterproof roll with high temperature resistance, high puncture strength, high wear resistance, high strength and high toughness can be prepared. The present invention is the first time that ultra-high molecular weight polyethylene is used as the main resin material, and is processed into a rollable sheet waterproof material by an efficient and green extrusion process, and is introduced into the field of building waterproofing, so that the high temperature resistance, high strength, puncture resistance, high wear resistance and high toughness of ultra-high molecular weight polyethylene can be used in underground and roof building waterproofing applications.
[0088] The present invention uses ultra-high molecular weight polyethylene resin with a molecular weight of 800,000-9 million to reduce the thickness of the coiled material by 10-50%, and the strength performance is equivalent to that of HDPE, which not only saves materials and reduces the burden on buildings, but is also of great significance to building energy conservation and emission reduction; at the same time, it improves the softness of the waterproof coiled material and the convenience of construction, which is of great significance to the improvement of the quality of waterproof construction.
[0089] The present invention develops a series of waterproof membranes and auxiliary materials based on ultra-high molecular weight polyethylene through the structural design of waterproof membranes. The membranes have the advantages of high temperature resistance, high puncture strength, high wear resistance, high strength and high toughness, thus improving the performance level of building waterproof materials.
[0090] Other features and advantages of the present invention will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0091] The above and other objects, features and advantages of the present invention will become more apparent through a more detailed description of exemplary embodiments of the present invention in conjunction with the accompanying drawings, wherein like reference numerals generally represent like components throughout the exemplary embodiments of the present invention.
[0092] Figure 1 A schematic diagram of the eccentric rotor of the dual-axis eccentric rotor extrusion plasticizing subsystem of the extrusion plasticizing molding system provided in Example 1 of the present invention is shown.
[0093] Figure 2 A side view of a sheet forming die of a high-density polyethylene extrusion system in the prior art is shown.
[0094] Figure 3 A side view of a sheet forming die of the extrusion plasticizing forming system provided in Example 1 of the present invention is shown.
[0095] Figure 4 A schematic diagram of the extrusion plasticizing molding system provided in Example 1 of the present invention is shown.
[0096] Figure 5 A front view of a sheet forming die of the extrusion plasticizing forming system provided in Example 1 of the present invention is shown.
[0097] FIG. 6( a ) is a schematic diagram showing the flow of UHMW-PE melt out of the film lip of the sheet forming die of the extrusion plasticizing forming system provided in Example 1 of the present invention.
[0098] FIG6( b ) is a schematic diagram showing the flow of PE melt out of the film lip of the sheet forming die of the extrusion plasticizing molding system provided in Example 1 of the present invention.
[0099] The following are the descriptions of the reference numerals:
[0100] 1-pointed die lip, 2-flat structure die lip, 3-melt pump, 4-sheet forming mold, 5-three-roll calendering equipment, 6-sheet winding device, 7-electric heating heat source, 8-temperature sensor socket, F-melt extrusion film lip force, D-melt flow direction, 9-UHMW-PE melt, 10-PE melt. DETAILED DESCRIPTION
[0101] The preferred embodiments of the present invention will be described in more detail below. Although the preferred embodiments of the present invention are described below, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided to make the present invention more thorough and complete, and to fully convey the scope of the present invention to those skilled in the art.
[0102] In the following embodiments and comparative examples:
[0103] The viscosity average molecular weight is measured using GB / T 1632.3-2010 (test method for determining viscosity of dilute polymer solutions using capillary viscometer).
[0104] Example 1
[0105] This embodiment provides an ultra-high molecular weight polyethylene resin sheet, wherein the raw material of the sheet is an ultra-high molecular weight polyethylene resin with a viscosity average molecular weight of 1.78 million;
[0106] The viscosity average molecular weight of the sheet is 1.65 million, that is, the viscosity average molecular weight of the sheet is reduced by 7.3% relative to the ultra-high molecular weight polyethylene resin of 1.78 million, and is not less than 90% of the viscosity average molecular weight of the ultra-high molecular weight polyethylene resin, that is, the viscosity average molecular weight retention rate of the sheet is more than 90%;
[0107] The thickness of the sheet is 0.3 mm.
[0108] The sheet is made by an extrusion plasticizing system, which includes a barrel, a double-shaft eccentric rotor extrusion plasticizing subsystem, a sheet forming die, a three-roll calendering device 5 and a sheet winding device 6;
[0109] The double-shaft eccentric rotor extrusion plasticizing subsystem comprises two mutually meshing eccentric rotors and a stator, wherein the eccentric rotor comprises a plurality of eccentric spiral structures and eccentric cylindrical structures, such as Figure 1 As shown in Table 2, each eccentric rotor includes a feeding section, a melt plasticizing section and a melt conveying section which are sequentially connected from the feeding end to the discharging end;
[0110] The feeding section includes a pre-feeding section, a first connecting section, a non-eccentric threaded rotor and a second connecting section connected in sequence; the pre-feeding section corresponds to T45-24-Q8-0A; the first connecting section and the second connecting section both correspond to T45-G10DP-0A; the non-eccentric threaded rotor corresponds to 4 T45-40-D40-0A;
[0111] The melt-plasticization section comprises a first melt-plasticization section, a second melt-plasticization section and a third melt-plasticization section connected in sequence, each melt-plasticization section comprises a first rotor assembly section with a gradually decreasing pitch, a straight extrusion reinforcement section and a reflux section connected in sequence; each melt-plasticization section is connected by a third connecting section;
[0112] The first rotor combination section with gradually decreasing pitch of the first melting and plasticizing section corresponds to a combination section composed of five pitch sections, namely T45-36-P36-0A, T45-32-P32-0A, T45-24-P24-0A, T45-40-P20-0A and T45-30-P15-0A, and there are 3 T45-36-P36-0A, 2 T45-32-P32-0A, 1 T45-24-P24-0A, 4 T45-40-P20-0A and 3 T45-30-P15-0A.
[0113] The first rotor combination section with gradually decreasing pitch of the second melting and plasticizing section corresponds to a combination section composed of four pitch sections: T45-32-P32-0A, T45-24-P24-0A, T45-40-P20-0A and T45-30-P15-0A, and there are 2 T45-32-P32-0A; 1 T45-24-P24-0A; 3 T45-40-P20-0A; and 1 T45-30-P15-0A.
[0114] The first rotor combination section with gradually decreasing pitch of the third melting and plasticizing section corresponds to a combination section composed of four pitch sections: T45-36-P36-0A, T45-32-P32-0A, T45-40-P20-0A and T45-30-P15-0A, and there are 2 T45-36-P36-0A; 1 T45-32-P32-0A; 3 T45-40-P20-0A; and 1 T45-30-P15-0A.
[0115] The straight extrusion reinforcement section corresponds to 3 T45-30-KP180-3-0A;
[0116] The reflux section corresponds to one T45-30-KP180-3-0B.
[0117] The third connection segment corresponds to T45-24-P8-0A;
[0118] The melt conveying section includes a melt conveying section 1, a melt conveying section 2 and a second rotor assembly section with a gradually decreasing pitch connected in sequence; the melt conveying section 1 and the melt conveying section 2 both correspond to T45-24-P8-0A;
[0119] The second rotor combination section with gradually decreasing pitch corresponds to a combination section composed of four pitch sections: T45-36-P36-0A, T45-24-P24-0A, T45-40-P20-0A and T45-30-P15-0A, and there are 2 T45-36-P36-0A; 1 T45-24-P24-0A; 2 T45-40-P20-0A; and 4 T45-30-P15-0A.
[0120] The die lip of the sheet forming die 4 is a flat die lip 2, and the thickness of the flat die lip 2 perpendicular to the sheet extrusion direction is 6 cm;
[0121] The sheet forming mold is provided with an electric heating source 7 and a plurality of temperature sensors, the plurality of temperature sensors are arranged in a direction parallel to the die lip, the electric heating source 7 and the plurality of temperature sensors are connected to realize zoned heating in the flow channel of the sheet forming mold; Figure 5As shown, through the electric heating heat source 7 and the multiple temperature sensors, multiple areas are obtained, each area has a temperature sensor socket 8, so that the temperature setting of area 5-1 and area 5-5 is higher than that of the central area 5-3, and the temperature of the sub-central area 5-2 and the sub-central area 5-4 is between the middle. The mold has the function of zone heating, which further solves the problem that the UHMW-PE melt affects the fluidity in the flow channel due to uneven temperature. In this embodiment, the temperature of area 5-1 and area 5-5 is 180°C, the temperature of the sub-central area 5-2 and the sub-central area 5-4 is 170°C, and the temperature of the central area 5-3 is 160°C.
[0122] The distance between the die lip of the sheet forming die and the three-roll calendering device is 50-100 mm;
[0123] The preparation method of the sheet comprises: feeding the raw material of the sheet from the feeding section into the double-axis eccentric rotor extrusion plasticizing subsystem, and after extrusion plasticizing in the first rotor combination section with gradually decreasing pitch and the straight extrusion reinforcement section, the reflux section generates material to strengthen extrusion plasticizing and compaction; finally, the melt is fed into the sheet forming die after achieving uniformity of melt temperature, pressure and plasticizing degree through the melt conveying section; the melt coming out of the die lip of the sheet forming die is subjected to three-roller calendering and winding treatment to obtain the sheet (UHMW-PE).
[0124] The head temperature of the double-shaft eccentric rotor extrusion plasticizing subsystem is 180°C, and the temperature of each section is 180-190°C;
[0125] The extrusion rate of the double-shaft eccentric rotor extrusion plasticizing subsystem is 3.5kg / min;
[0126] The eccentric rotor speed of the double-shaft eccentric rotor extrusion plasticizing subsystem is 180-220 rpm;
[0127] The temperature of the three-roll calendering equipment is 90°C.
[0128] Example 2-3
[0129] Embodiments 2-3 respectively provide an ultra-high molecular weight polyethylene resin sheet, and the difference between Embodiments 2-3 and Embodiment 1 is that:
[0130] The thickness of the sheet of Example 2 was 0.5 mm.
[0131] The thickness of the sheet of Example 3 was 1.0 mm.
[0132] Example 4
[0133] This embodiment provides a self-adhesive ultra-high molecular weight polyethylene waterproofing membrane, comprising an ultra-high molecular weight polyethylene resin sheet (Example 1), an upper self-adhesive layer (1.0 mm self-adhesive butyl adhesive) and an isolation film arranged in sequence from top to bottom.
[0134] Example 5
[0135] The present embodiment provides a pre-laid reverse-adhesive ultra-high molecular weight waterproof membrane, comprising a lower self-adhesive layer (0.3 mm self-adhesive butyl adhesive), an ultra-high molecular weight polyethylene resin sheet (Example 2), a styrene-butylene block copolymer type polymer hot-melt pressure-sensitive adhesive layer and a weather-resistant polyacrylate type anti-stick coating, which are arranged in sequence from top to bottom.
[0136] The total thickness of the styrene-butylene block copolymer type high molecular hot-melt pressure-sensitive adhesive layer and the weather-resistant polyacrylate type anti-stick coating is 0.3 mm;
[0137] Comparative Example 1
[0138] This comparative example provides a high-density polyethylene (HDPE) waterproof sheet, which is produced by single-screw extrusion of HDPE 5000S resin produced by Sinopec.
[0139] Comparative Example 2
[0140] This comparative example uses a high shear force grinding disc mechanochemical reactor to process an ultra-high molecular weight polyethylene resin with a viscosity average molecular weight of 1.8 million. As the number of grindings increases, its melt flow index gradually increases. After 30 grindings, the melt flow index increases from the initial 0 to 0.101g / 10min, and the viscosity average molecular weight decreases by 46%. (Zou Huawei. Research on the influence of stress-induced reaction on the rheological behavior and properties of polymers. Sichuan: Sichuan University, 2005)
[0141] Test Example 1
[0142] This test example tests the physical properties of the materials of Examples 1-3 and Comparative Example 1, and the results are shown in Table 3. Among them:
[0143] The test methods for tensile strength, elongation at break and right-angle tear refer to
[0144] GB / T18173.1-2013JS2 resin type sheet.
[0145] The test method for puncture resistance refers to GB / T 23457-2017 Pre-laid waterproofing membrane.
[0146] The test method for wear resistance refers to GB / T1768-2006, rubber grinding wheel model CS-17, load 750g, 500 revolutions.
[0147] Table 3
[0148]
[0149]
[0150] Test Example 2
[0151] In this test example, the physical performance data of the self-adhesive ultra-high molecular weight polyethylene waterproof membrane of Example 4 was tested. The results are shown in Table 4 below. The test was based on the test method of GB / T 328.21-2007 for shear performance of polymer waterproof membrane joints and 5.12.2 for bonding membrane to aluminum plate in GB23441-2009.
[0152] Table 4 Adhesion performance of self-adhesive ultra-high molecular weight polyethylene waterproof membrane (N / mm)
[0153] Coil and Coil Coil and sheet Membrane and cement board 2.3 2.7 3.6
[0154] Test Example 3
[0155] In this test example, the physical performance data of the pre-laid reverse-adhesive ultra-high molecular weight waterproof membrane of Example 5 was tested. The results are shown in Table 5 below. The test is based on GB / T 23457-2007.
[0156] Table 5 Bonding performance of pre-laid reverse-adhesive ultra-high molecular weight waterproof membrane and post-cast concrete (N / mm)
[0157] No treatment Heat Treatment UV treatment 28 days of immersion 3.3 2.7 3.6 3.8
[0158] The viscosity average molecular weight retention rate is of great significance to the performance of the sheet. The excellent performance of ultra-high molecular weight polyethylene resin is due to the entanglement between the ultra-long molecular chains, which makes the sheet have excellent impact resistance, high temperature resistance, low temperature resistance and wear resistance.
[0159] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.
Claims
1. An ultra-high molecular weight polyethylene resin sheet, characterized in that: The raw material of the sheet includes ultra-high molecular weight polyethylene resin with a viscosity average molecular weight of 800,000 to 9,000,000; The viscosity average molecular weight of the sheet is not less than 80% of the viscosity average molecular weight of the ultra-high molecular weight polyethylene resin; Preferably, the thickness of the sheet is 0.1-2.0 mm.
2. The ultra-high molecular weight polyethylene resin sheet according to claim 1, wherein The raw materials of the sheet include ultra-high molecular weight polyethylene resin with a viscosity average molecular weight of 800,000 to 9 million, other polymer resins, processing aids and pigments and fillers; and based on the total weight of the sheet, the content of the ultra-high molecular weight polyethylene resin with a viscosity average molecular weight of 800,000 to 9 million is 55-100%, and the total content of other polymer resins, processing aids and pigments and fillers is 0-45%.
3. The ultra-high molecular weight polyethylene resin sheet according to claim 2, wherein The sheet is made by an extrusion plasticizing system, which includes a barrel, a double-shaft eccentric rotor extrusion plasticizing subsystem, a sheet forming die, a three-roll calendering device and a sheet winding device; The double-shaft eccentric rotor extrusion plasticizing subsystem comprises two mutually meshing eccentric rotors and a stator, wherein the eccentric rotor comprises a plurality of eccentric spiral structures and eccentric cylindrical structures, including a feed section, a melt plasticizing section and a melt conveying section sequentially connected from a feed end to a discharge end; The feed section comprises a non-eccentric threaded rotor; The melt plasticizing section comprises a first rotor assembly section, a straight extrusion reinforcement section and a reflux section which are connected in sequence and gradually decrease in pitch; The melt conveying section comprises a melt conveying section 1, a melt conveying section 2 and a second rotor assembly section with a gradually decreasing pitch which are connected in sequence; The spiral direction of the reflux section is opposite to that of the other sections of the eccentric rotor.
4. The ultra-high molecular weight polyethylene resin sheet according to claim 3, wherein The eccentric rotor has a diameter of 20-120 mm, a compression ratio of 2-2.8:1, and an aspect ratio of 38-45:1; The melt plasticizing section and the melt conveying section are multiple sections, and the number of sections, lengths and the aspect ratio of the rotor combination are determined according to the viscosity average molecular weight of the ultra-high molecular weight polyethylene resin.
5. The ultra-high molecular weight polyethylene resin sheet according to claim 2, wherein The die lip of the sheet forming die is a flat die lip, and the thickness of the flat die lip perpendicular to the sheet extrusion direction is 2-20 cm; The sheet forming mold is provided with an electric heating heat source and a plurality of temperature sensors, the plurality of temperature sensors are arranged in a direction parallel to the die lip, the electric heating heat source and the plurality of temperature sensors are connected to realize zoned heating in the flow channel of the sheet forming mold; The distance between the die opening of the sheet forming die and the three-roll calendering device is 5-300 mm.
6. The ultra-high molecular weight polyethylene resin sheet according to any one of claims 1 to 5, wherein The preparation method of the sheet material comprises: feeding the raw material of the sheet material from the feeding section into the double-axis eccentric rotor extrusion plasticizing subsystem, and after extrusion plasticizing in the first rotor combination section with gradually decreasing pitch and the straight extrusion reinforcement section, the material reflux is generated in the reflux section to strengthen the extrusion plasticizing and compaction; finally, the raw material of the sheet material is fed into the sheet forming die after achieving uniformity of melt temperature, pressure and plasticizing degree through the melt conveying section; the melt coming out of the die lip of the sheet forming die is subjected to three-roller calendering and winding treatment to obtain the sheet material.
7. The ultra-high molecular weight polyethylene resin sheet according to claim 6, wherein The temperature of each section of the eccentric rotor of the double-shaft eccentric rotor extrusion plasticizing subsystem is set to be lower than 240°C, preferably 160-220°C; The extrusion rate of the double-shaft eccentric rotor extrusion plasticizing subsystem is 0.2-12kg / min; The rotation speed of the eccentric rotor of the double-shaft eccentric rotor extrusion plasticizing subsystem is 5-300 rpm; The temperature of the three-roll calendering equipment is 20-200°C, preferably 70°C-150°C.
8. A method for preparing an ultra-high molecular weight polyethylene resin sheet according to any one of claims 1 to 7, characterized in that: The preparation method is carried out in the extrusion plasticizing and molding system, comprising: feeding the raw material of the sheet into the double-axis eccentric rotor extrusion plasticizing subsystem from the feeding section, and after extrusion plasticizing in the first rotor combination section with gradually decreasing pitch and the straight extrusion reinforcement section, the material reflux is generated by the reflux section to strengthen the extrusion plasticizing and compaction; finally, the melt is fed into the sheet molding die after achieving uniformity of melt temperature, pressure and plasticizing degree through the melt conveying section; the melt coming out of the die lip of the sheet molding die is subjected to three-roller calendering and winding treatment to obtain the sheet.
9. Use of the ultra-high molecular weight polyethylene resin sheet according to any one of claims 1 to 7 in waterproofing rolls.
10. A waterproof roll material, characterized in that: The waterproof coiled material comprises an ultra-high molecular weight polyethylene resin sheet and a functional layer arranged on the upper surface of the ultra-high molecular weight polyethylene resin sheet; The ultra-high molecular weight polyethylene resin sheet is the ultra-high molecular weight polyethylene resin sheet according to any one of claims 1 to 7; The functional layer includes a hot melt adhesive layer and a weather-resistant anti-stick coating; the ultra-high molecular weight polyethylene resin sheet, the hot melt adhesive layer and the weather-resistant anti-stick coating are arranged in sequence from top to bottom; or, the functional layer is at least one of a PVDF film, a PVF film and a weather-resistant metal foil coated with a weather-resistant coating; or, the functional layer is an upper self-adhesive layer; Optionally, the lower surface of the ultra-high molecular weight polyethylene resin sheet is provided with a lower self-adhesive layer; Preferably, the thickness of the hot melt adhesive layer is 0.2-1.5 mm; Preferably, the thickness of the upper self-adhesive layer and the lower self-adhesive layer is independently 0.2-1.5 mm.