Environment-friendly printing corrugated carton and preparation method thereof
Through the combination technology of modified adhesive and wear-resistant oil, the wear resistance and service life of corrugated cartons are improved, and the problem of poor wear resistance on the surface of existing corrugated cartons is solved, achieving stronger bonding and more durable surface protection.
Patent Information
- Application Number
- CN202411079085.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The surface of existing corrugated cartons has poor wear resistance and are prone to friction damage within the printing, which affects the service life.
Using a combination technology of modified adhesive and wear-resistant oil, the modified adhesive consists of components such as starch, borax, glycerin and formamide, which enhances adhesion and stability through cross-linking reaction and complex formation; Polymethyl methacrylate and acrylonitrile-styrene-acrylate terpolymer are added to the wear-resistant oil to form a hard protective film.
It significantly improves the overall structural strength and wear resistance of corrugated cardboard, extends service life, and maintains the transparency and appearance quality of printed handwriting.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of corrugated paper preparation, and relates to an environmentally friendly printed corrugated paper box and a preparation method thereof. Background Art
[0002] Corrugated boxes have gradually replaced wooden boxes and other transport packaging containers with their superior performance and good processing performance, becoming the main force of transport packaging; in addition to protecting goods and facilitating storage and transportation, they also play a role in beautifying and promoting goods; corrugated boxes are green and environmentally friendly products, which are beneficial to the environment and convenient for loading and unloading and transportation; in order to achieve the purpose of environmental protection, the prior art uses recycled paper as the raw material of corrugated boxes, but the surface wear resistance of the corrugated boxes produced in the prior art is poor, and the content printed on the surface is easily damaged by friction. Summary of the invention
[0003] The object of the present invention is to provide an environmentally friendly printed corrugated paper box and a preparation method thereof, which has the characteristics of wear resistance and long service life.
[0004] The purpose of the present invention can be achieved through the following technical solutions:
[0005] An environmentally friendly printed corrugated paper box, the corrugated paper box includes a base paper, a corrugated paper core and a face paper from the inside to the outside, the three are bonded by a modified adhesive, and a layer of wear-resistant varnish is attached to the surface of the face paper, wherein the preparation method of the modified adhesive is as follows:
[0006] S11: weigh 50-60% starch, 20-30% deionized water, 5-10% glycerol, 3-7% formamide, 2-3% borax, 2-3% diacetyl tartaric acid monoglyceride, and 0.5-1% defoaming agent in percentage by mass;
[0007] S12: Put starch into a blender, add deionized water according to the formula ratio, stir at a speed of 200 to 300 r / min for 0.5 to 1 h, and ultrasonicate for 0.5 h to obtain a uniformly mixed starch solution A;
[0008] S13: adding borax and diacetyl tartaric acid monoglyceride to starch solution A according to the formula ratio, stirring at a speed of 150 to 200 r / min for 0.5 to 1 h to obtain a mixed solution B;
[0009] S14: adding glycerol, formamide and defoaming agent to the mixed solution B according to the formula ratio, and continuing to stir at a speed of 150 to 200 r / min for 0.5 to 1 h to obtain a mixed solution C;
[0010] S15: placing the mixed solution C into a homogenizer and homogenizing it at 5-7 MPa for 0.5 h to obtain the modified adhesive;
[0011] Wherein, the defoaming agent is one or more of diethanolamine, distearylethylenediamine, isopropyl alcohol and lauroyl isopropylamine.
[0012] Furthermore, the preparation method of the wear-resistant varnish is as follows:
[0013] S21: dissolving polymethyl methacrylate in ethyl acetate to obtain a mixed solution with a mass fraction of 30%, adding 1wt% acrylonitrile-styrene-acrylate terpolymer, heating to 40°C, and stirring at a speed of 300 r / min for 1 h to obtain a mixed solution D;
[0014] S22: Add 2 wt % of fumed silica to the mixed solution D, and stir at a speed of 400 r / min for 0.5 h to obtain the wear-resistant varnish.
[0015] A method for preparing an environmentally friendly printed corrugated paper box, the method for preparing the environmentally friendly printed corrugated paper box is specifically as follows:
[0016] S31: The recycled waste paper is purged with nitrogen, and the purged waste paper is frozen at -10°C for 4 hours. After freezing, the waste paper is put into a ball mill for crushing at a speed of 300 r / min. The crushed paper is soaked in 80°C water for 12 hours to soften, and filtered;
[0017] S32: putting the paper obtained after softening and filtering into a pulping machine for kneading and grinding treatment, the speed of the pulping machine is 1450r / min, the treatment time is 2h, and a uniform paper paste is obtained;
[0018] S33: adding 2 wt % of urea-formaldehyde resin to the paper paste, stirring at a speed of 400 r / min for 2 h to obtain paper pulp;
[0019] S34: putting the pulp into a paper machine for dehydration and pressing to form a flat paperboard;
[0020] S35: putting the pulp into a corrugated paper core making machine, and making a corrugated paper core having a concave and convex corrugated shape through heating, pressurizing and forming processes;
[0021] S36: Using a modified adhesive to stick flat cardboard on both sides of the corrugated paper core to obtain corrugated cardboard, spraying a layer of wear-resistant varnish on the surface of the face paper, drying it using a laser drying method, and then using a molding machine to mold the corrugated cardboard. After the molding process, let it stand for 12 hours to obtain the environmentally friendly printed corrugated paper box.
[0022] Furthermore, the purge rate of nitrogen in S31 is 10 m / s.
[0023] Furthermore, in S34, the pressure of the paper machine is 10 MPa and the temperature is 80°C.
[0024] Furthermore, in S35, the pressure is 7 MPa and the temperature is 80°C.
[0025] Furthermore, the spraying parameters of the wear-resistant varnish in S36 are a spraying distance of 60 mm and a spraying rate of 50 mm / s.
[0026] Furthermore, the parameters of the laser drying in S36 are: laser power 200 W, temperature 80° C., and irradiation time 40 min.
[0027] The modified adhesive is used in the present invention, and the viscosity of the adhesive is improved, so that the overall structural strength of the corrugated paperboard is improved. When the bonding between the face plate and the core plate is more firm, the cushioning performance of the corrugated paperboard is improved, so that the corrugated paperboard can better absorb and disperse energy when impacted. When the bonding strength between the face plate and the core plate is high enough, the corrugated paperboard can better maintain its integrity during the recycling process, which is convenient for reprocessing and reuse.
[0028] The modified adhesive of the present invention uses starch as the main raw material. Starch is a natural polysaccharide, and the hydroxyl hydrophilic groups on its molecular chain give starch natural bonding properties, which is in line with the concept of green environmental protection; borax, as a cross-linking agent, undergoes a cross-linking reaction with the hydroxyl hydrophilic groups on the starch molecular chain to form a borate ester chemical bond, thereby enhancing the interaction between starch molecules, which improves the adhesion of the adhesive and makes the interlayer bonding of the corrugated board more firm; diacetyl tartaric acid monoglyceride forms a complex with starch molecules to prevent starch from swelling and loss, improves the gelatinization properties of starch, and thus enhances the stability and bonding properties of the adhesive; glycerol, as a plasticizer, can react with starch molecules through the hydroxyl groups in its molecules The hydroxyl groups in the starch molecules form hydrogen bond interactions, thereby improving the flexibility and fluidity of the adhesive, facilitating uniform coating of the adhesive during the production of corrugated cardboard and reducing the problem of uneven coating; formamide is also a plasticizer, and the amino groups in formamide will also form strong hydrogen bonds with the hydroxyl groups in the starch molecules. At the same time, formamide, as a small molecule plasticizer, can enter the starch molecules and destroy the crystalline structure of the starch, thereby reducing the glass transition temperature of the adhesive, improving its flexibility, making it better adapt to the deformation of the corrugated cardboard, and improving the bonding effect; the addition of the defoamer effectively suppresses the foam generated during the stirring and homogenization process, improves the stability of the adhesive, and avoids the influence of bubbles on the bonding effect.
[0029] In order to further improve the service life of the corrugated paper box, the present invention adds a layer of wear-resistant varnish on the surface of the corrugated paper panel. The polymethyl methacrylate and acrylonitrile-styrene-acrylate (ASA) terpolymer in the wear-resistant varnish are both polymers with excellent wear resistance. When the wear-resistant varnish is coated on the surface of the corrugated paper and dried and cured, a hard protective film is formed. This film can effectively resist friction and wear, thereby extending the service life of the corrugated paper.
[0030] Among them, PMMA, as the main component of wear-resistant varnish, has high light transmittance and will not affect the printed words on the surface of corrugated paper. The high light transmittance of PMMA comes from the low absorption and high transmittance of light by the C=O bond and CH bond in its molecular structure. The PMMA molecular chain also has excellent flexibility, which enables it to undergo certain deformation when impacted and is not easy to break.
[0031] The acrylic rubber component in the acrylonitrile-styrene-acrylate (ASA) terpolymer is evenly dispersed in the acrylonitrile-styrene copolymer matrix in the form of particles. This structure makes the ASA copolymer have excellent wear resistance. The ASA copolymer also has excellent weather resistance and can resist the effects of environmental factors such as ultraviolet rays and temperature changes on corrugated paper. Adding ASA copolymer to the wear-resistant varnish can extend the service life of corrugated paper and maintain its appearance and performance stability.
[0032] As a nano-scale filler, fumed silica can significantly improve the wear resistance of wear-resistant varnish; increase the hardness of the material, making the surface of corrugated paper more durable.
[0033] The wear-resistant varnish of the present invention can also fill the tiny depressions and unevenness on the surface of the corrugated paper during the coating and curing process, thereby making the paper surface smoother and flatter. This improvement not only improves the appearance quality of the corrugated paper, but also facilitates subsequent processing and treatment.
[0034] Beneficial effects of the present invention:
[0035] The present invention uses a modified adhesive, which uses starch as a main raw material, adds borax as a cross-linking agent, glycerol and formamide as plasticizers, and diacetyl tartaric acid monoglyceride forms a complex with starch molecules to improve the viscosity of the adhesive, thereby improving the overall structural strength of the corrugated paperboard, and the modified adhesive in the present invention complies with the concept of green environmental protection;
[0036] The present invention adds a layer of wear-resistant varnish on the surface of the corrugated paper panel. The polymethyl methacrylate and acrylonitrile-styrene-acrylate terpolymer in the wear-resistant varnish are both polymers with excellent wear resistance. When the wear-resistant varnish is coated on the surface of the corrugated paper and dried and solidified, a hard protective film is formed. This film can effectively resist friction and wear, thereby extending the service life of the corrugated paper. DETAILED DESCRIPTION
[0037] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with the embodiments.
[0038] Example 1
[0039] The preparation method of the modified adhesive is as follows:
[0040] S11: weigh, by mass percentage, 60% starch, 20% deionized water, 7% glycerol, 7% formamide, 3% borax, 2% diacetyl tartaric acid monoglyceride, and 1% diethanolamine;
[0041] S12: Put starch into a blender, add deionized water according to the formula ratio, stir at a speed of 200 r / min for 1 hour, and ultrasonicate for 0.5 hour to obtain a uniformly mixed starch solution A;
[0042] S13: adding borax and diacetyl tartaric acid monoglyceride to starch solution A according to the formula ratio, stirring at a speed of 150 r / min for 1 hour to obtain a mixed solution B;
[0043] S14: adding glycerol, formamide and diethanolamine to the mixed solution B according to the formula ratio, and continuing to stir at a speed of 150 r / min for 1 hour to obtain a mixed solution C;
[0044] S15: placing the mixed solution C into a homogenizer and homogenizing it at 5 MPa for 0.5 h to obtain the modified adhesive;
[0045] The preparation method of the wear-resistant varnish is as follows:
[0046] S21: dissolving polymethyl methacrylate in ethyl acetate to obtain a mixed solution with a mass fraction of 30%, adding 1wt% acrylonitrile-styrene-acrylate terpolymer, heating to 40°C, and stirring at a speed of 300 r / min for 1 h to obtain a mixed solution D;
[0047] S22: adding 2 wt % of fumed silica to the mixed solution D, stirring at a speed of 400 r / min for 0.5 h to obtain the wear-resistant varnish;
[0048] The preparation method of the environmentally friendly printed corrugated paper box is as follows:
[0049] S31: The recycled waste paper is purged with nitrogen at a purging rate of 10 m / s. The purged waste paper is frozen at -10°C for 4 hours. After freezing, the waste paper is put into a ball mill for crushing at a speed of 300 r / min. The crushed paper is soaked in water at 80°C for 12 hours to soften, and filtered.
[0050] S32: putting the paper obtained after softening and filtering into a pulping machine for kneading and grinding treatment, the speed of the pulping machine is 1450r / min, the treatment time is 2h, and a uniform paper paste is obtained;
[0051] S33: adding 2 wt % of urea-formaldehyde resin to the paper paste, wherein the urea-formaldehyde resin in the present invention is purchased from Hubei Jianchu Biopharmaceutical Co., Ltd., with a product number of HWG21059, and stirring at a speed of 400 r / min for 2 h to obtain paper pulp;
[0052] S34: putting the pulp into a paper machine for dehydration and pressing to form a flat paperboard, the pressure of the paper machine is 10 MPa and the temperature is 80° C.;
[0053] S35: putting the pulp into a corrugated paper core making machine at a pressure of 7 MPa and a temperature of 80° C., and undergoing heating, pressurizing, and forming processes to make a corrugated paper core having a concave-convex corrugated shape;
[0054] S36: Use modified adhesive to stick flat cardboard on both sides of the corrugated paper core to obtain corrugated cardboard, spray a layer of wear-resistant varnish on the surface of the face paper, the spraying parameters are spraying distance 60mm, spraying rate 50mm / s, and after drying by laser drying method, the laser drying parameters are laser power 200W, temperature 80℃, irradiation time 40min, and then use a molding machine to mold the corrugated cardboard. After lamination post-treatment, let it stand for 12h to obtain the environmentally friendly printed corrugated paper box.
[0055] Example 2
[0056] The preparation method of the modified adhesive is as follows:
[0057] S11: weigh, by mass percentage, 50% starch, 30% deionized water, 7% glycerol, 7% formamide, 2% borax, 3% diacetyl tartaric acid monoglyceride, and 1% distearyl ethylenediamine;
[0058] S12: Put starch into a blender, add deionized water according to the formula ratio, stir at a speed of 300 r / min for 0.5 h, and ultrasonicate for 0.5 h to obtain a uniformly mixed starch solution A;
[0059] S13: adding borax and diacetyl tartaric acid monoglyceride to starch solution A according to the formula ratio, stirring at a speed of 200 r / min for 0.5 h to obtain a mixed solution B;
[0060] S14: adding glycerol, formamide and distearylethylenediamine to the mixed solution B according to the formula ratio, and continuing to stir at a speed of 200 r / min for 0.5 h to obtain a mixed solution C;
[0061] S15: placing the mixed solution C into a homogenizer and homogenizing it at 7 MPa for 0.5 h to obtain the modified adhesive;
[0062] The preparation method of the wear-resistant varnish is as follows:
[0063] S21: dissolving polymethyl methacrylate in ethyl acetate to obtain a mixed solution with a mass fraction of 30%, adding 1wt% acrylonitrile-styrene-acrylate terpolymer, heating to 40°C, and stirring at a speed of 300 r / min for 1 h to obtain a mixed solution D;
[0064] S22: adding 2 wt % of fumed silica to the mixed solution D, stirring at a speed of 400 r / min for 0.5 h to obtain the wear-resistant varnish;
[0065] The preparation method of the environmentally friendly printed corrugated paper box is as follows:
[0066] S31: The recycled waste paper is purged with nitrogen at a purging rate of 10 m / s. The purged waste paper is frozen at -10°C for 4 hours. After freezing, the waste paper is put into a ball mill for crushing at a speed of 300 r / min. The crushed paper is soaked in water at 80°C for 12 hours to soften, and filtered.
[0067] S32: putting the paper obtained after softening and filtering into a pulping machine for kneading and grinding treatment, the speed of the pulping machine is 1450r / min, the treatment time is 2h, and a uniform paper paste is obtained;
[0068] S33: adding 2 wt % of urea-formaldehyde resin to the paper paste, stirring at a speed of 400 r / min for 2 h to obtain paper pulp;
[0069] S34: putting the pulp into a paper machine for dehydration and pressing to form a flat paperboard, the pressure of the paper machine is 10 MPa and the temperature is 80° C.;
[0070] S35: putting the pulp into a corrugated paper core making machine at a pressure of 7 MPa and a temperature of 80° C., and undergoing heating, pressurizing, and forming processes to make a corrugated paper core having a concave-convex corrugated shape;
[0071] S36: Use modified adhesive to stick flat cardboard on both sides of the corrugated paper core to obtain corrugated cardboard, spray a layer of wear-resistant varnish on the surface of the face paper, the spraying parameters are spraying distance 60mm, spraying rate 50mm / s, and after drying by laser drying method, the laser drying parameters are laser power 200W, temperature 80℃, irradiation time 40min, and then use a molding machine to mold the corrugated cardboard. After lamination post-treatment, let it stand for 12h to obtain the environmentally friendly printed corrugated paper box.
[0072] Example 3
[0073] The preparation method of the modified adhesive is as follows:
[0074] S11: weigh 57% starch, 30% deionized water, 5% glycerol, 3% formamide, 2% borax, 2.5% diacetyl tartaric acid monoglyceride, and 0.5% isopropyl alcohol in percentage by mass;
[0075] S12: Put starch into a blender, add deionized water according to the formula ratio, stir at a speed of 200 r / min for 0.5 h, and ultrasonicate for 0.5 h to obtain a uniformly mixed starch solution A;
[0076] S13: adding borax and diacetyl tartaric acid monoglyceride to starch solution A according to the formula ratio, stirring at a speed of 150 r / min for 1 hour to obtain a mixed solution B;
[0077] S14: adding glycerol, formamide and isopropanol to the mixed solution B according to the formula ratio, and continuing to stir at a speed of 150 r / min for 1 hour to obtain a mixed solution C;
[0078] S15: placing the mixed solution C into a homogenizer and homogenizing it at 5 MPa for 0.5 h to obtain the modified adhesive;
[0079] The preparation method of the wear-resistant varnish is as follows:
[0080] S21: dissolving polymethyl methacrylate in ethyl acetate to obtain a mixed solution with a mass fraction of 30%, adding 1wt% acrylonitrile-styrene-acrylate terpolymer, heating to 40°C, and stirring at a speed of 300 r / min for 1 h to obtain a mixed solution D;
[0081] S22: adding 2 wt % of fumed silica to the mixed solution D, stirring at a speed of 400 r / min for 0.5 h to obtain the wear-resistant varnish;
[0082] The preparation method of the environmentally friendly printed corrugated paper box is as follows:
[0083] S31: The recycled waste paper is purged with nitrogen at a purging rate of 10 m / s. The purged waste paper is frozen at -10°C for 4 hours. After freezing, the waste paper is put into a ball mill for crushing at a speed of 300 r / min. The crushed paper is soaked in water at 80°C for 12 hours to soften, and filtered.
[0084] S32: putting the paper obtained after softening and filtering into a pulping machine for kneading and grinding treatment, the speed of the pulping machine is 1450r / min, the treatment time is 2h, and a uniform paper paste is obtained;
[0085] S33: adding 2 wt % of urea-formaldehyde resin to the paper paste, stirring at a speed of 400 r / min for 2 h to obtain paper pulp;
[0086] S34: putting the pulp into a paper machine for dehydration and pressing to form a flat paperboard, the pressure of the paper machine is 10 MPa and the temperature is 80° C.;
[0087] S35: putting the pulp into a corrugated paper core making machine at a pressure of 7 MPa and a temperature of 80° C., and undergoing heating, pressurizing, and forming processes to make a corrugated paper core having a concave-convex corrugated shape;
[0088] S36: Use modified adhesive to stick flat cardboard on both sides of the corrugated paper core to obtain corrugated cardboard, spray a layer of wear-resistant varnish on the surface of the face paper, the spraying parameters are spraying distance 60mm, spraying rate 50mm / s, and after drying by laser drying method, the laser drying parameters are laser power 200W, temperature 80℃, irradiation time 40min, and then use a molding machine to mold the corrugated cardboard. After lamination post-treatment, let it stand for 12h to obtain the environmentally friendly printed corrugated paper box.
[0089] Example 4
[0090] The preparation method of the modified adhesive is as follows:
[0091] S11: weigh 55% starch, 25% deionized water, 10% glycerol, 5% formamide, 2% borax, 2% diacetyl tartaric acid monoglyceride, and 1% lauroyl isopropanolamine in percentage by mass;
[0092] S12: Put starch into a blender, add deionized water according to the formula ratio, stir at a speed of 200 r / min for 0.5 h, and ultrasonicate for 0.5 h to obtain a uniformly mixed starch solution A;
[0093] S13: adding borax and diacetyl tartaric acid monoglyceride to starch solution A according to the formula ratio, stirring at a speed of 150 r / min for 1 hour to obtain a mixed solution B;
[0094] S14: adding glycerol, formamide and lauroyl isopropanolamine to the mixed solution B according to the formula ratio, and continuing to stir at a speed of 150 r / min for 1 h to obtain a mixed solution C;
[0095] S15: placing the mixed solution C into a homogenizer and homogenizing it at 5 MPa for 0.5 h to obtain the modified adhesive;
[0096] The preparation method of the wear-resistant varnish is as follows:
[0097] S21: dissolving polymethyl methacrylate in ethyl acetate to obtain a mixed solution with a mass fraction of 30%, adding 1wt% acrylonitrile-styrene-acrylate terpolymer, heating to 40°C, and stirring at a speed of 300 r / min for 1 h to obtain a mixed solution D;
[0098] S22: adding 2 wt % of fumed silica to the mixed solution D, stirring at a speed of 400 r / min for 0.5 h to obtain the wear-resistant varnish;
[0099] The preparation method of the environmentally friendly printed corrugated paper box is as follows:
[0100] S31: The recycled waste paper is purged with nitrogen at a purging rate of 10 m / s. The purged waste paper is frozen at -10°C for 4 hours. After freezing, the waste paper is put into a ball mill for crushing at a speed of 300 r / min. The crushed paper is soaked in water at 80°C for 12 hours to soften, and filtered.
[0101] S32: putting the paper obtained after softening and filtering into a pulping machine for kneading and grinding treatment, the speed of the pulping machine is 1450r / min, the treatment time is 2h, and a uniform paper paste is obtained;
[0102] S33: adding 2 wt % of urea-formaldehyde resin to the paper paste, stirring at a speed of 400 r / min for 2 h to obtain paper pulp;
[0103] S34: putting the pulp into a paper machine for dehydration and pressing to form a flat paperboard, the pressure of the paper machine is 10 MPa and the temperature is 80° C.;
[0104] S35: putting the pulp into a corrugated paper core making machine at a pressure of 7 MPa and a temperature of 80° C., and undergoing heating, pressurizing, and forming processes to make a corrugated paper core having a concave-convex corrugated shape;
[0105] S36: Use modified adhesive to stick flat cardboard on both sides of the corrugated paper core to obtain corrugated cardboard, spray a layer of wear-resistant varnish on the surface of the face paper, the spraying parameters are spraying distance 60mm, spraying rate 50mm / s, and after drying by laser drying method, the laser drying parameters are laser power 200W, temperature 80℃, irradiation time 40min, and then use a molding machine to mold the corrugated cardboard. After lamination post-treatment, let it stand for 12h to obtain the environmentally friendly printed corrugated paper box.
[0106] Comparative Example 1
[0107] In this comparative example, glycerol was not added to the modified adhesive, and the remaining steps were consistent with those in Example 1.
[0108] Comparative Example 2
[0109] In this comparative example, formamide was not added to the modified adhesive, and the remaining steps were consistent with those in Example 1.
[0110] Comparative Example 3
[0111] In this comparative example, borax is not added to the modified adhesive, and the remaining steps are consistent with those of Example 1.
[0112] Comparative Example 4
[0113] In this comparative example, diacetyl tartaric acid monoglyceride is not added to the modified adhesive, and the remaining steps are consistent with those of Example 1.
[0114] Comparative Example 5
[0115] In this comparative example, no wear-resistant varnish is added to the surface of the face paper, and the remaining steps are consistent with those of Example 1.
[0116] Comparative Example 6
[0117] In this comparative example, acrylonitrile-styrene-acrylate terpolymer is not added to the wear-resistant varnish on the surface of the face paper, and the remaining steps are consistent with those of Example 1.
[0118] The adhesive strength test of the peeling of the face paper and the corrugated paper core was carried out on Examples 1 to 4 and Comparative Examples 1 to 4 according to GB / T 6544-2008.
[0119] Adhesion strength (N / m) Example 1 1620 Example 2 1580 Example 3 1600 Example 4 1600 Comparative Example 1 1200 Comparative Example 2 1100 Comparative Example 3 950 Comparative Example 4 1200
[0120] The experimental data show that the addition of glycerol, formamide, borax, and diacetyl tartaric acid monoglyceride in the modified adhesive improves the bonding strength of the adhesive and the overall structural strength of the corrugated paper.
[0121] The surface wear and scratch resistance of Example 1 and Comparative Examples 5 to 6 were tested according to the GB / T6739-2006 pencil hardness test. The pencil was fixed on the device and pressed down on the panel surface at a 45° angle under a load of 500g. The hardness decreased from 3H to 3B. The hardness of the pen tip when a 3mm scratch appeared was recorded, and the scratch resistance was scored.
[0122] Cut the sample into 270*60mm and fix it on the friction table of the equipment; then fix a piece of white paper on a 4-pound load block and place it above the sample, set the friction times to 600 times, 800 times, 1000 times, and 1200 times respectively, and observe the limit number of times when scratches begin to appear after friction;
[0123] Scratch resistance test (3H-3B) Wear test number (limit number) Example 1 2H 1000 Comparative Example 5 B 600 Comparative Example 6 H 800
[0124] Experimental data show that adding a layer of wear-resistant varnish on the panel surface effectively improves the wear and scratch resistance of the corrugated paper surface, making the corrugated paper surface more durable.
[0125] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. An environmentally friendly printed corrugated paper box, characterized in that: The corrugated paper box includes bottom paper, corrugated paper core and face paper from inside to outside, and the three are bonded by modified adhesive, and a layer of wear-resistant varnish is attached to the surface of the face paper, wherein the preparation method of the modified adhesive is as follows: S11: weigh 50-60% starch, 20-30% deionized water, 5-10% glycerol, 3-7% formamide, 2-3% borax, 2-3% diacetyl tartaric acid monoglyceride, and 0.5-1% defoaming agent in percentage by mass; S12: Put starch into a blender, add deionized water according to the formula ratio, stir at a speed of 200 to 300 r / min for 0.5 to 1 h, and ultrasonicate for 0.5 h to obtain a uniformly mixed starch solution A; S13: adding borax and diacetyl tartaric acid monoglyceride to starch solution A according to the formula ratio, stirring at a speed of 150 to 200 r / min for 0.5 to 1 h to obtain a mixed solution B; S14: adding glycerol, formamide and defoaming agent to the mixed solution B according to the formula ratio, and continuing to stir at a speed of 150 to 200 r / min for 0.5 to 1 h to obtain a mixed solution C; S15: placing the mixed solution C into a homogenizer and homogenizing it at 5-7 MPa for 0.5 h to obtain the modified adhesive; Wherein, the defoaming agent is one or more of diethanolamine, distearylethylenediamine, isopropyl alcohol and lauroyl isopropylamine.
2. The environmentally friendly printed corrugated paper box according to claim 1, characterized in that: The preparation method of the wear-resistant varnish is as follows: S21: dissolving polymethyl methacrylate in ethyl acetate to obtain a mixed solution with a mass fraction of 30%, adding 1wt% acrylonitrile-styrene-acrylate terpolymer, heating to 40°C, and stirring at a speed of 300 r / min for 1 h to obtain a mixed solution D; S22: Add 2 wt % of fumed silica to the mixed solution D, and stir at a speed of 400 r / min for 0.5 h to obtain the wear-resistant varnish.
3. A method for preparing an environmentally friendly printed corrugated paper box according to any one of claims 1 to 2, characterized in that: The preparation method of the environmentally friendly printed corrugated paper box is as follows: S31: The recycled waste paper is purged with nitrogen, and the purged waste paper is frozen at -10°C for 4 hours. After freezing, the waste paper is put into a ball mill for crushing at a speed of 300 r / min. The crushed paper is soaked in 80°C water for 12 hours to soften, and filtered; S32: putting the paper obtained after softening and filtering into a pulping machine for kneading and grinding treatment, the speed of the pulping machine is 1450r / min, the treatment time is 2h, and a uniform paper paste is obtained; S33: adding 2 wt % of urea-formaldehyde resin to the paper paste, stirring at a speed of 400 r / min for 2 h to obtain paper pulp; S34: putting the pulp into a paper machine for dehydration and pressing to form a flat paperboard; S35: putting the pulp into a corrugated paper core making machine, and making a corrugated paper core having a concave and convex corrugated shape through heating, pressurizing and forming processes; S36: Using a modified adhesive to stick flat cardboard on both sides of the corrugated paper core to obtain corrugated cardboard, spraying a layer of wear-resistant varnish on the surface of the face paper, drying it using a laser drying method, and then using a molding machine to mold the corrugated cardboard. After the molding process, let it stand for 12 hours to obtain the environmentally friendly printed corrugated paper box.
4. The method for preparing an environmentally friendly printed corrugated paper box according to claim 3, characterized in that: The purge rate of nitrogen in S31 is 10 m / s.
5. The method for preparing an environmentally friendly printed corrugated paper box according to claim 3, characterized in that: The pressure of the paper machine in S34 is 10 MPa and the temperature is 80°C.
6. The method for preparing an environmentally friendly printed corrugated paper box according to claim 3, characterized in that: The pressure in S35 is 7 MPa and the temperature is 80°C.
7. The method for preparing an environmentally friendly printed corrugated paper box according to claim 3, characterized in that: The spraying parameters of the wear-resistant varnish in S36 are a spraying distance of 60 mm and a spraying rate of 50 mm / s.
8. The method for preparing an environmentally friendly printed corrugated paper box according to claim 3, characterized in that: The parameters of the laser drying in S36 are: laser power 200 W, temperature 80° C., and irradiation time 40 min.
Citation Information
Patent Citations
Composite material and preparation method thereof
CN106519530A
Preparation method of adhesive
CN106554731A
Green high-precision flexible printing corrugated carton
CN107600614A
ASA / PMMA resin composition and preparation method thereof
CN109651743A
High-strength anti-deformation corrugated paper box and production technology
CN110106733A