Preparation process of manganous-manganic oxide precursor based on ammonium sulfate system

By using ammonium sulfate roasting leaching method and two-step iron removal method in high-ferromagnetic rhombic acid, the problems of low manganese extraction efficiency and difficult to remove iron impurities in high-ferromagnetic rhombic acid are solved, efficient manganese recycling and iron removal are achieved, and the product is improved Purity and resource utilization.

CN118993154AActive Publication Date: 2024-11-22HUNAN SHUANGFU NEW MATERIAL TECH CO LTD

Patent Information

Application Number
CN202411482116.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-23
Publication Date
2024-11-22
Estimated Expiration
2044-10-23

AI Technical Summary

Technical Problem

The prior art is difficult to efficiently extract trimanium tetraoxide precursors from high-ferrous rhombic ore, and there are problems with impurities and impurities and wastewater, especially the low iron removal rate, which affects manganese recycling efficiency and product purity.

Method used

Using ammonium sulfate-based roasting leaching method, pretreatment of high-ferrous rhomanganite powder with urea and thiourea, after roasting, ammonium sulfate is used for refining and extraction, combined with two-step iron removal method (water immersion and oxidation precipitation method) to improve manganese recovery rate and iron removal rate.

Benefits of technology

Efficient manganese recycling and iron removal have been achieved. The total recovery rate of manganese reaches 92.82%, and the total removal rate of iron reaches 99.64%, which significantly improves product purity and resource utilization, and has the advantages of economical and environmental protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention relates to the technical field of metallurgy, in particular to a preparation process of a manganous-manganic oxide precursor based on an ammonium sulfate system. The preparation process comprises the following steps: (1) crushing; (2) pretreatment; (3) roasting; (4) leaching; (5) removing impurities; (6) precipitating manganese; and (7) oxidizing to obtain the manganous-manganic oxide precursor. The high-iron rhodochrosite is treated through the technology, efficient recovery of manganese and efficient removal of iron are achieved, the technology has the advantages of being efficient and environmentally friendly, the total recovery rate of manganese reaches 92.82%, the total removal rate of iron reaches 99.64%, and the product purity and the resource utilization rate are remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metallurgy, and in particular to a process for preparing a manganese tetraoxide precursor based on an ammonium sulfate system. Background Art

[0002] As an important inorganic material, manganese tetraoxide (Mn3O4) has special physical and chemical properties that make it an important component in the preparation of battery materials. In the preparation of battery materials, manganese tetraoxide is used as a precursor and can be converted into the final battery material after further processing and treatment. Specifically, manganese tetraoxide is a precursor of spinel lithium manganate, and this structure is of great significance for improving the performance and stability of batteries. Therefore, the quality and purity of the manganese tetraoxide precursor have a decisive influence on the performance of the final battery.

[0003] The precursor of manganese tetraoxide is usually obtained by processing manganese ore. Common manganese minerals in nature are: pyroxenite, hausmannite, bare iron ore and rhodochrosite. As the most economical manganese oxide ore, pyroxenite is gradually depleted in high-grade deposits due to its large-scale mining. High-iron rhodochrosite is one of the main types of manganese ore in my country, and its industrial reserves account for more than one-tenth of the manganese industry. However, due to the high iron and sulfur content of this manganese ore and the low manganese content, it has not been fully utilized.

[0004] At present, the most common manganese ore processing technologies are wet reduction leaching, roasting leaching and microbial reduction leaching. The basic principle of wet reduction is to mix manganese ore with a reducing agent and carry out leaching reaction in an acidic environment. Although wet reduction can achieve a higher extraction efficiency, the addition of a reducing agent will introduce impurity elements, increase the difficulty of manganese recovery, and produce a large amount of wastewater. The roasting leaching process is to roast under the conditions of adding a solid reducing agent or through a reducing gas to reduce the high-valent manganese oxide to manganese oxide, and then use an acid solution to leach and extract manganese. Compared with wet reduction, roasting leaching is more economical. Microbial reduction leaching is considered to be an environmentally friendly method, but its leaching rate is very slow, usually requiring 6-8 days.

[0005] The ammonium sulfate roasting leaching process is a further improvement of the roasting leaching process. The principle is to convert the metal in the manganese ore into ammonium sulfate salts, and then extract it efficiently through the water leaching process. The ammonium sulfate roasting leaching process is a method that can achieve both valuable metal recovery and environmental protection at the same time, and is considered to be a promising process. However, there is no report on the use of this process to extract manganese from high-iron rhodochrosite. Summary of the invention

[0006] In view of this, the purpose of the present invention is to propose a process for preparing a manganese tetraoxide precursor based on an ammonium sulfate system, and to effectively prepare a low-impurity manganese tetraoxide precursor from high-iron rhodochrosite by an ammonium sulfate roasting and leaching method.

[0007] Based on the above purpose, the present invention provides a process for preparing a manganese tetraoxide precursor based on an ammonium sulfate system, comprising the following steps: (1) Crushing: crushing the high-iron rhodochrosite ore and grinding it through a 80-100 mesh sieve to obtain high-iron rhodochrosite ore powder; (2) Pretreatment: Add the high-iron rhodochrosite powder, urea and thiourea prepared in step (1) into deionized water, stir at 75-80° C. until it becomes a sticky paste, and then dry and grind to obtain doped ore powder; (3) Calcination: ammonium sulfate and the doped ore powder prepared in step (2) are mixed, spread on a crucible, placed in a tube furnace, and air is introduced. The temperature in the tube furnace is raised to 190-210° C. at a rate of 8-12° C. / min, kept at that temperature for 25-35 min, then raised to 390-410° C. at a rate of 4-6° C. / min, kept at that temperature for 100-140 min, and cooled to room temperature to obtain a calcined ore powder; (4) Leaching: adding the calcined powder prepared in step (3) into deionized water, heating to 65-75°C, stirring for 40-80 minutes, filtering at normal pressure to obtain a filtrate, which is the leachate; (5) impurity removal: add hydrogen peroxide to the leachate prepared in step (4), heat to 55-65°C, stir for 40-80 min, then adjust the pH to 4.9-5.1 with industrial ammonia water, let stand for 4-8 h, filter at normal pressure, take the filtrate, add sodium diethyldithiocarbamate trihydrate to the filtrate, heat to 60-80°C, stir for 20-40 min, let stand for 10-14 h, filter at normal pressure, then add ammonium fluoride, heat to 80-95°C, stir for 50-60 min, let stand for 10-14 h, filter at normal pressure to obtain a manganese-rich solution; (6) Manganese precipitation: adjust the pH of the manganese-rich solution prepared in step (5) to 9.8-10.5 using aqueous ammonia, raise the temperature to 55-65°C, stir for 50-70 minutes, let stand for 10-14 hours to precipitate manganese, filter under normal pressure, and dry the filter cake to obtain the manganese precipitate; (7) Oxidation: Add the manganese precipitate prepared in step (4) into deionized water and stir for 20-40 min. Then add industrial ammonia water to adjust the pH value to 9.5-10.5. Then add hydrazine hydrate and react for 7-9 h. After the reaction is completed, filter, wash and dry at 70-80° C. for 3-5 h to obtain a trimanganese tetraoxide precursor.

[0008] Furthermore, in the step (2), the weight ratio of the high iron rhodochrosite powder, urea and thiourea is 1:0.18-0.22:0.04-0.06.

[0009] Furthermore, the amount of ammonium sulfate added in step (3) is 1.7-1.9 times the weight of the high-iron rhodochrosite powder in the doped ore powder.

[0010] Preferably, the amount of ammonium sulfate added in step (3) is 1.8 times the weight of the high-iron rhodochrosite powder in the doped ore powder. Furthermore, in step (3), the end of the tube furnace is connected to a gas collecting bottle, and the liquid in the gas collecting bottle is a 1 mol / L sulfuric acid solution.

[0011] Furthermore, in step (3), the air flow rate is 0.8-1.2 L / min.

[0012] Furthermore, in step (5), the amount of hydrogen peroxide added to the leaching solution is 15-25 ml / L.

[0013] Preferably, in step (5), the amount of hydrogen peroxide added to the leaching solution is 20 ml / L.

[0014] Furthermore, in step (5), the amount of sodium diethyldithiocarbamate trihydrate added to the leachate is 0.13-0.16 g / L.

[0015] Preferably, in step (5), the amount of sodium diethyldithiocarbamate trihydrate added to the leachate is 0.15 g / L.

[0016] Furthermore, in step (5), the amount of ammonium fluoride added to the leaching solution is 4-4.5 g / L.

[0017] Preferably, in step (5), the amount of ammonium fluoride added to the leaching solution is 4.2 g / L.

[0018] Beneficial effects of the present invention: The present invention proposes a process for preparing a manganese tetraoxide precursor based on an ammonium sulfate system. By treating high-iron rhodochrosite ore through the process, efficient recovery of manganese and efficient removal of iron are achieved. The process has the characteristics of high efficiency and environmental protection. The total recovery rate of manganese reaches 92.82%, and the total removal rate of iron reaches 99.64%, which significantly improves product purity and resource utilization. The method not only excels in economy and environmental protection, but also provides reliable technical support and improvement space for industrial production.

[0019] The invention uses urea and thiourea to treat high-iron rhodochrosite powder before ammonium sulfate roasting and leaching, and the urea and thiourea are adsorbed in the pores of the high-iron rhodochrosite powder. During the ammonium sulfate roasting process, the high-iron rhodochrosite can be effectively refined and the roasting atmosphere can be optimized, thereby effectively improving the recovery rate of manganese. Meanwhile, the generated yttroclase is insoluble in water and can be removed by water leaching, thereby improving the removal rate of iron impurities.

[0020] The invention adopts two steps to remove iron, the first step is to remove iron by water immersion using ferroaluminate method, and the second step is to remove iron by oxidation precipitation method. Through the two-step iron removal, the removal rate of iron impurities is greatly improved. DETAILED DESCRIPTION

[0021] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.

[0022] The contents of various elements in the high-iron rhodochrosite in the examples of the present invention and the comparative examples are shown in Table 1: Table 1 Element content of high iron rhodochrosite

[0023] Embodiment 1: (1) Crushing: crushing the high-iron rhodochrosite ore and grinding it through a 100-mesh sieve to obtain high-iron rhodochrosite ore powder; (2) Pretreatment: 1 kg of the high-iron rhodochrosite powder prepared in step (1), 0.2 kg of urea and 0.05 kg of thiourea were added to 10 L of deionized water, stirred at 80 ° C until it became a sticky paste, and then dried and ground to obtain doped ore powder; (3) Calcination: 1.8 kg of ammonium sulfate and the doped ore powder prepared in step (2) were mixed, spread on a crucible, placed in a tubular furnace, and air was introduced at an air flow rate of 1 L / min. A gas collecting bottle was connected to the end of the tubular furnace, and the liquid in the gas collecting bottle was 1 mol / L sulfuric acid solution. The temperature in the tubular furnace was raised to 200°C at a rate of 10°C / min, kept at that temperature for 30 min, then raised to 400°C at a rate of 5°C / min, kept at that temperature for 120 min, and cooled to room temperature to obtain a calcined ore powder; (4) Leaching: add the calcined powder prepared in step (3) into 10 L of deionized water, heat to 70°C, stir for 60 min, filter at normal pressure to obtain a filtrate, which is the leachate; (5) Impurity removal: add 200 mL of 30% hydrogen peroxide to the leachate prepared in step (4), heat to 60°C, stir for 60 min, adjust the pH to 5.0 with industrial ammonia water, let stand for 6 h to precipitate iron and aluminum impurities, filter at normal pressure, take the filtrate, add 1.5 g of sodium diethyldithiocarbamate trihydrate to the filtrate, heat to 70°C, stir for 30 min, let stand for 12 h to precipitate heavy metal impurities, filter at normal pressure, add 42 g of ammonium fluoride, heat to 90°C, stir for 60 min, let stand for 12 h to precipitate magnesium impurities, filter at normal pressure to obtain a manganese-rich solution; (6) Manganese precipitation: adjust the pH of the manganese-rich solution prepared in step (5) to 10 using aqueous ammonia, raise the temperature to 60° C., stir for 60 min, let stand for 12 h to precipitate manganese, filter under normal pressure, and dry the filter cake to obtain the manganese precipitate; (7) Oxidation: The manganese precipitate prepared in step (4) was added into 3 L of deionized water and stirred for 30 min. Then, industrial ammonia water was added to adjust the pH value to 10. Then, 15 mL of hydrazine hydrate was added and the reaction was carried out for 8 h. After the reaction was completed, the mixture was filtered, washed, and dried at 80 °C for 4 h to obtain a manganese tetraoxide precursor.

[0024] Embodiment 2: (1) Crushing: crushing the high-iron rhodochrosite ore and grinding it through an 80-mesh sieve to obtain high-iron rhodochrosite ore powder; (2) Pretreatment: 1 kg of the high-iron rhodochrosite powder prepared in step (1), 0.18 kg of urea and 0.04 kg of thiourea were added to 10 L of deionized water, stirred at 75 ° C until it became a sticky paste, and then dried and ground to obtain doped ore powder; (3) Calcination: 1.7 kg of ammonium sulfate and the doped ore powder prepared in step (2) were mixed, spread on a crucible, placed in a tubular furnace, and air was introduced at an air flow rate of 0.8 L / min. A gas collecting bottle was connected to the end of the tubular furnace, and the liquid in the gas collecting bottle was 1 mol / L sulfuric acid solution. The temperature in the tubular furnace was raised to 190°C at 8°C / min, kept at this temperature for 25 min, then raised to 390°C at 4°C / min, kept at this temperature for 100 min, and cooled to room temperature to obtain a calcined ore powder; (4) Leaching: add the calcined powder prepared in step (3) into 10 L of deionized water, heat to 65° C., stir for 40 min, filter at normal pressure to obtain a filtrate, which is the leachate; (5) Impurity removal: add 150 mL of 30% hydrogen peroxide to the leachate prepared in step (4), heat to 55°C, stir for 40 min, adjust the pH to 4.9 with industrial ammonia water, let stand for 4 h to precipitate iron and aluminum impurities, filter at normal pressure, take the filtrate, add 1.3 g of sodium diethyldithiocarbamate trihydrate to the filtrate, heat to 60°C, stir for 20 min, let stand for 10 h to precipitate heavy metal impurities, filter at normal pressure, add 40 g of ammonium fluoride, heat to 80°C, stir for 50 min, let stand for 10 h to precipitate magnesium impurities, filter at normal pressure to obtain a manganese-rich solution; (6) Manganese precipitation: adjust the pH of the manganese-rich solution prepared in step (5) to 9.8 with ammonia water, raise the temperature to 55° C., stir for 50 min, let stand for 10 h to precipitate manganese, filter under normal pressure, and dry the filter cake to obtain the manganese precipitate; (7) Oxidation: The manganese precipitate prepared in step (4) was added into 3 L of deionized water and stirred for 20 min. Industrial ammonia water was then added to adjust the pH value to 19.5. Then 15 mL of hydrazine hydrate was added and the reaction was continued for 7 h. After the reaction was completed, the mixture was filtered, washed and dried at 70 °C for 5 h to obtain a manganese tetraoxide precursor.

[0025] Embodiment 3: (1) Crushing: crushing the high-iron rhodochrosite ore and grinding it through a 100-mesh sieve to obtain high-iron rhodochrosite ore powder; (2) Pretreatment: 1 kg of the high-iron rhodochrosite powder prepared in step (1), 0.22 kg of urea and 0.06 kg of thiourea were added to 10 L of deionized water, stirred at 80 ° C until it became a sticky paste, and then dried and ground to obtain doped ore powder; (3) Calcination: 1.9 kg of ammonium sulfate and the doped ore powder prepared in step (2) were mixed, spread on a crucible, placed in a tubular furnace, and air was introduced at an air flow rate of 1.2 L / min. A gas collecting bottle was connected to the end of the tubular furnace. The liquid in the gas collecting bottle was 1 mol / L sulfuric acid solution. The temperature in the tubular furnace was raised to 210°C at a rate of 12°C / min, kept at that temperature for 40 min, then raised to 410°C at a rate of 6°C / min, kept at that temperature for 140 min, and cooled to room temperature to obtain a calcined ore powder; (4) Leaching: add the calcined powder prepared in step (3) into 10 L of deionized water, heat to 75°C, stir for 80 min, filter at normal pressure to obtain a filtrate, which is the leachate; (5) Impurity removal: add 250 mL of 30% hydrogen peroxide to the leachate prepared in step (4), heat to 65°C, stir for 80 min, adjust the pH to 5.1 with industrial ammonia water, let stand for 8 h to precipitate iron and aluminum impurities, filter at normal pressure, take the filtrate, add 1.6 g of sodium diethyldithiocarbamate trihydrate to the filtrate, heat to 80°C, stir for 40 min, let stand for 14 h to precipitate heavy metal impurities, filter at normal pressure, add 45 g of ammonium fluoride, heat to 95°C, stir for 60 min, let stand for 14 h to precipitate magnesium impurities, filter at normal pressure to obtain a manganese-rich solution; (6) Manganese precipitation: adjust the pH of the manganese-rich solution prepared in step (5) to 10.5 using aqueous ammonia, raise the temperature to 65° C., stir for 70 min, let stand for 14 h to precipitate manganese, filter under normal pressure, and dry the filter cake to obtain the manganese precipitate; (7) Oxidation: The manganese precipitate prepared in step (4) was added into 3 L of deionized water and stirred for 40 min. Then, industrial ammonia water was added to adjust the pH value to 10.5. Then, 15 mL of hydrazine hydrate was added and the reaction was carried out for 8 h. After the reaction was completed, the mixture was filtered, washed, and dried at 80 °C for 3 h to obtain a manganese tetraoxide precursor.

[0026] Comparative Example 1: The difference between Comparative Example 1 and Example 1 is that no urea is added in step (2); The specific steps are as follows: (1) Crushing: crushing the high-iron rhodochrosite ore and grinding it through a 100-mesh sieve to obtain high-iron rhodochrosite ore powder; (2) Pretreatment: 1 kg of the high-iron rhodochrosite powder prepared in step (1) and 0.05 kg of thiourea were added to 10 L of deionized water, stirred at 80 ° C until it became a sticky paste, and then dried and ground to obtain doped ore powder; (3) Calcination: 1.8 kg of ammonium sulfate and the doped ore powder prepared in step (2) were mixed, spread on a crucible, placed in a tubular furnace, and air was introduced at an air flow rate of 1 L / min. A gas collecting bottle was connected to the end of the tubular furnace, and the liquid in the gas collecting bottle was 1 mol / L sulfuric acid solution. The temperature in the tubular furnace was raised to 200°C at a rate of 10°C / min, kept at that temperature for 30 min, then raised to 400°C at a rate of 5°C / min, kept at that temperature for 120 min, and cooled to room temperature to obtain a calcined ore powder; (4) Leaching: add the calcined powder prepared in step (3) into 10 L of deionized water, heat to 70°C, stir for 60 min, filter at normal pressure to obtain a filtrate, which is the leachate; (5) Impurity removal: add 200 mL of 30% hydrogen peroxide to the leachate prepared in step (4), heat to 60°C, stir for 60 min, adjust the pH to 5.0 with industrial ammonia water, let stand for 6 h to precipitate iron and aluminum impurities, filter at normal pressure, take the filtrate, add 1.5 g of sodium diethyldithiocarbamate trihydrate to the filtrate, heat to 70°C, stir for 30 min, let stand for 12 h to precipitate heavy metal impurities, filter at normal pressure, add 42 g of ammonium fluoride, heat to 90°C, stir for 60 min, let stand for 12 h to precipitate magnesium impurities, filter at normal pressure to obtain a manganese-rich solution; (6) Manganese precipitation: adjust the pH of the manganese-rich solution prepared in step (5) to 10 using aqueous ammonia, raise the temperature to 60° C., stir for 60 min, let stand for 12 h to precipitate manganese, filter under normal pressure, and dry the filter cake to obtain the manganese precipitate; (7) Oxidation: The manganese precipitate prepared in step (4) was added into 3 L of deionized water and stirred for 30 min. Then, industrial ammonia water was added to adjust the pH value to 10. Then, 15 mL of hydrazine hydrate was added and the reaction was carried out for 8 h. After the reaction was completed, the mixture was filtered, washed, and dried at 80 °C for 4 h to obtain a manganese tetraoxide precursor.

[0027] Comparative Example 2: The difference between Comparative Example 2 and Example 1 is that no thiourea is added in step (2); The specific steps are as follows: (1) Crushing: crushing the high-iron rhodochrosite ore and grinding it through a 100-mesh sieve to obtain high-iron rhodochrosite ore powder; (2) Pretreatment: 1 kg of the high-iron rhodochrosite powder prepared in step (1) and 0.2 kg of urea were added to 10 L of deionized water, stirred at 80° C. until it became a sticky paste, and then dried and ground to obtain doped ore powder; (3) Calcination: 1.8 kg of ammonium sulfate and the doped ore powder prepared in step (2) were mixed, spread on a crucible, placed in a tubular furnace, and air was introduced at an air flow rate of 1 L / min. A gas collecting bottle was connected to the end of the tubular furnace, and the liquid in the gas collecting bottle was 1 mol / L sulfuric acid solution. The temperature in the tubular furnace was raised to 200°C at a rate of 10°C / min, kept at that temperature for 30 min, then raised to 400°C at a rate of 5°C / min, kept at that temperature for 120 min, and cooled to room temperature to obtain a calcined ore powder; (4) Leaching: add the calcined powder prepared in step (3) into 10 L of deionized water, heat to 70°C, stir for 60 min, filter at normal pressure to obtain a filtrate, which is the leachate; (5) Impurity removal: add 200 mL of 30% hydrogen peroxide to the leachate prepared in step (4), heat to 60°C, stir for 60 min, adjust the pH to 5.0 with industrial ammonia water, let stand for 6 h to precipitate iron and aluminum impurities, filter at normal pressure, take the filtrate, add 1.5 g of sodium diethyldithiocarbamate trihydrate to the filtrate, heat to 70°C, stir for 30 min, let stand for 12 h to precipitate heavy metal impurities, filter at normal pressure, add 42 g of ammonium fluoride, heat to 90°C, stir for 60 min, let stand for 12 h to precipitate magnesium impurities, filter at normal pressure to obtain a manganese-rich solution; (6) Manganese precipitation: adjust the pH of the manganese-rich solution prepared in step (5) to 10 using aqueous ammonia, raise the temperature to 60° C., stir for 60 min, let stand for 12 h to precipitate manganese, filter under normal pressure, and dry the filter cake to obtain the manganese precipitate; (7) Oxidation: The manganese precipitate prepared in step (4) was added into 3 L of deionized water and stirred for 30 min. Then, industrial ammonia water was added to adjust the pH value to 10. Then, 15 mL of hydrazine hydrate was added and the reaction was carried out for 8 h. After the reaction was completed, the mixture was filtered, washed, and dried at 80 °C for 4 h to obtain a manganese tetraoxide precursor.

[0028] Comparative Example 3: Comparative Example 3 differs from Example 1 in that: there is no pretreatment in step (2); The specific steps are as follows: (1) Crushing: crushing the high-iron rhodochrosite ore and grinding it through a 100-mesh sieve to obtain high-iron rhodochrosite ore powder; (2) Calcination: 1.8 kg of ammonium sulfate and the high-iron rhodochrosite powder prepared in step (1) were mixed, spread on a crucible, placed in a tubular furnace, and air was introduced at an air flow rate of 1 L / min. A gas collecting bottle was connected to the end of the tubular furnace, and the liquid in the gas collecting bottle was 1 mol / L sulfuric acid solution. The temperature in the tubular furnace was raised to 200°C at a rate of 10°C / min, kept at that temperature for 30 min, then raised to 400°C at a rate of 5°C / min, kept at that temperature for 120 min, and cooled to room temperature to obtain a calcined ore powder; (3) Leaching: add the calcined powder prepared in step (2) into 10 L of deionized water, heat to 70°C, stir for 60 min, filter at normal pressure to obtain a filtrate, which is the leachate; (4) Impurity removal: add 200 mL of 30% hydrogen peroxide to the leachate prepared in step (3), heat to 60°C, stir for 60 min, adjust the pH to 5.0 with industrial ammonia water, let stand for 6 h to precipitate iron and aluminum impurities, filter at normal pressure, take the filtrate, add 1.5 g of sodium diethyldithiocarbamate trihydrate to the filtrate, heat to 70°C, stir for 30 min, let stand for 12 h to precipitate heavy metal impurities, filter at normal pressure, add 42 g of ammonium fluoride, heat to 90°C, stir for 60 min, let stand for 12 h to precipitate magnesium impurities, filter at normal pressure to obtain a manganese-rich solution; (5) Manganese precipitation: the pH of the manganese-rich solution prepared in step (4) is adjusted to 10 using aqueous ammonia, the temperature is raised to 60°C, stirred for 60 minutes, allowed to stand for 12 hours to precipitate manganese, filtered under normal pressure, and the filter cake is dried to obtain the manganese precipitate; (6) Oxidation: The manganese precipitate prepared in step (5) was added into 3 L of deionized water and stirred for 30 min. Then, industrial ammonia water was added to adjust the pH value to 10. Then, 15 mL of hydrazine hydrate was added and the reaction was carried out for 8 h. After the reaction was completed, the mixture was filtered, washed, and dried at 80 °C for 4 h to obtain a manganese tetraoxide precursor.

[0029] Comparative Example 4: The difference between Comparative Example 4 and Example 1 is that: in step (3), the temperature in the tube furnace is directly raised to 400° C. at a rate of 10° C. / min and kept at that temperature for 150 min; The specific steps are as follows: (1) Crushing: crushing the high-iron rhodochrosite ore and grinding it through a 100-mesh sieve to obtain high-iron rhodochrosite ore powder; (2) Pretreatment: 1 kg of the high-iron rhodochrosite powder prepared in step (1), 0.2 kg of urea and 0.05 kg of thiourea were added to 10 L of deionized water, stirred at 80 ° C until it became a sticky paste, and then dried and ground to obtain doped ore powder; (3) Calcination: 1.8 kg of ammonium sulfate and the doped ore powder prepared in step (2) were mixed, spread on a crucible, placed in a tubular furnace, and air was introduced at an air flow rate of 1 L / min. A gas collecting bottle was connected to the end of the tubular furnace, and the liquid in the gas collecting bottle was 1 mol / L sulfuric acid solution. The temperature in the tubular furnace was raised to 400°C at a rate of 10°C / min, kept at this temperature for 150 min, and cooled to room temperature to obtain a calcined ore powder; (4) Leaching: add the calcined powder prepared in step (3) into 10 L of deionized water, heat to 70°C, stir for 60 min, filter at normal pressure to obtain a filtrate, which is the leachate; (5) Impurity removal: add 200 mL of 30% hydrogen peroxide to the leachate prepared in step (4), heat to 60°C, stir for 60 min, adjust the pH to 5.0 with industrial ammonia water, let stand for 6 h to precipitate iron and aluminum impurities, filter at normal pressure, take the filtrate, add 1.5 g of sodium diethyldithiocarbamate trihydrate to the filtrate, heat to 70°C, stir for 30 min, let stand for 12 h to precipitate heavy metal impurities, filter at normal pressure, add 42 g of ammonium fluoride, heat to 90°C, stir for 60 min, let stand for 12 h to precipitate magnesium impurities, filter at normal pressure to obtain a manganese-rich solution; (6) Manganese precipitation: adjust the pH of the manganese-rich solution prepared in step (5) to 10 using aqueous ammonia, raise the temperature to 60° C., stir for 60 min, let stand for 12 h to precipitate manganese, filter under normal pressure, and dry the filter cake to obtain the manganese precipitate; (7) Oxidation: The manganese precipitate prepared in step (4) was added into 3 L of deionized water and stirred for 30 min. Then, industrial ammonia water was added to adjust the pH value to 10. Then, 15 mL of hydrazine hydrate was added and the reaction was carried out for 8 h. After the reaction was completed, the mixture was filtered, washed, and dried at 80 °C for 4 h to obtain a manganese tetraoxide precursor.

[0030] Comparative Example 5: The difference between Comparative Example 5 and Example 1 is that: no hydrogen peroxide is added in step (5); The specific steps are as follows: (1) Crushing: crushing the high-iron rhodochrosite ore and grinding it through a 100-mesh sieve to obtain high-iron rhodochrosite ore powder; (2) Pretreatment: 1 kg of the high-iron rhodochrosite powder prepared in step (1), 0.2 kg of urea and 0.05 kg of thiourea were added to 10 L of deionized water, stirred at 80 ° C until it became a sticky paste, and then dried and ground to obtain doped ore powder; (3) Calcination: 1.8 kg of ammonium sulfate and the doped ore powder prepared in step (2) were mixed, spread on a crucible, placed in a tubular furnace, and air was introduced at an air flow rate of 1 L / min. A gas collecting bottle was connected to the end of the tubular furnace, and the liquid in the gas collecting bottle was 1 mol / L sulfuric acid solution. The temperature in the tubular furnace was raised to 200°C at a rate of 10°C / min, kept at that temperature for 30 min, then raised to 400°C at a rate of 5°C / min, kept at that temperature for 120 min, and cooled to room temperature to obtain a calcined ore powder; (4) Leaching: add the calcined powder prepared in step (3) into 10 L of deionized water, heat to 70°C, stir for 60 min, filter at normal pressure to obtain a filtrate, which is the leachate; (5) Impurity removal: adjust the pH of the leachate prepared in step (4) to 5.0 with industrial ammonia water, let it stand for 6 hours to precipitate iron and aluminum impurities, filter at normal pressure, take the filtrate, add 1.5 g of sodium diethyldithiocarbamate trihydrate to the filtrate, heat it to 70°C, stir it for 30 minutes, let it stand for 12 hours to precipitate heavy metal impurities, filter it at normal pressure, then add 42 g of ammonium fluoride, heat it to 90°C, stir it for 60 minutes, let it stand for 12 hours to precipitate magnesium impurities, filter it at normal pressure to obtain a manganese-rich solution; (6) Manganese precipitation: adjust the pH of the manganese-rich solution prepared in step (5) to 10 using aqueous ammonia, raise the temperature to 60° C., stir for 60 min, let stand for 12 h to precipitate manganese, filter under normal pressure, and dry the filter cake to obtain the manganese precipitate; (7) Oxidation: The manganese precipitate prepared in step (4) was added into 3 L of deionized water and stirred for 30 min. Then, industrial ammonia water was added to adjust the pH value to 10. Then, 15 mL of hydrazine hydrate was added and the reaction was carried out for 8 h. After the reaction was completed, the mixture was filtered, washed, and dried at 80 °C for 4 h to obtain a manganese tetraoxide precursor.

[0031] The contents of manganese and iron in the trimanganese tetraoxide precursors of the embodiment and the comparative example were tested respectively, and the results are shown in Table 2.

[0032] Table 2 Manganese and iron content

[0033] According to the mass conservation rule, the total recovery rate of manganese and the total removal rate of iron in the embodiment and the comparative example were calculated respectively. The results are shown in Table 3.

[0034] Table 3 Total recovery rate of manganese and total removal rate of iron

[0035] Data Analysis: It can be seen from the data of Examples 1-3 in Table 2-3 that the use of the ammonium sulfate system-based manganese tetraoxide precursor preparation process of the present invention to treat high-iron rhodochrosite can achieve a total manganese recovery rate of up to 92.82% and a total iron removal rate of up to 99.64%.

[0036] It can be seen from the data of Example 1 and Comparative Examples 1-3 in Table 2-3 that the addition of urea and thiourea during the pretreatment process can effectively improve the manganese recovery rate and the iron removal rate. This may be because the small molecular urea and thiourea can be diffused and adsorbed in the pores of the high-iron rhodochrosite during the pretreatment process. In the later roasting process, they decompose and produce gas. The pressure of the gas helps to refine the high-iron rhodochrosite again. At the same time, the reducing ammonia and hydrogen sulfide produced can effectively reduce the high-valent manganese to generate water-soluble ammonium manganese sulfate, while promoting the formation of poorly water-soluble ferrocyanide, and inhibiting the formation of grass ferrocyanide with poor sedimentation performance and difficult to filter and wash, thereby achieving a high manganese recovery rate and iron removal rate.

[0037] It can be seen from the data of Example 1 and Comparative Example 4 in Table 2-3 that directly increasing the temperature to 400°C during the roasting process will lead to a decrease in the total recovery rate of manganese. This is mainly because the gradient heating helps to refine the high-iron rhodochrosite and maintain a reducing atmosphere.

[0038] It can be seen from the data of Example 1 and Comparative Example 5 in Table 2-3 that the addition of hydrogen peroxide during the impurity removal process is helpful for the removal of iron impurities. This is mainly because hydrogen peroxide can oxidize the valence state of iron impurities from divalent to trivalent, which is easier to precipitate.

[0039] The impurity contents of the trimanganese tetraoxide precursor prepared in the examples were tested respectively, and compared with the national standard GB / T 21836-2008 for the content of impurities in trimanganese tetraoxide. The results are shown in Table 4.

[0040] Table 4 Impurity content in manganese tetraoxide products

[0041] Note: Contents below 0.001 are uniformly indicated by “ / ”.

[0042] Data analysis: From the data of Examples 1-3 in Table 4, it can be seen that the impurity content of the trimanganese tetraoxide precursor prepared by the present invention meets the standard of the national standard GB / T 21836-2008, and the impurity content is relatively low, which provides favorable conditions for the preparation of high-performance and high-purity lithium manganate.

[0043] Those skilled in the art should understand that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of the present invention is limited to these examples. Under the concept of the present invention, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of the different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity.

Claims

1. A process for preparing a manganese tetraoxide precursor based on an ammonium sulfate system, characterized in that: The following steps are involved: (1) Crushing: crushing the high-iron rhodochrosite ore and grinding it through a 80-100 mesh sieve to obtain high-iron rhodochrosite ore powder; (2) Pretreatment: Add the high-iron rhodochrosite powder, urea and thiourea prepared in step (1) into deionized water, stir at 75-80° C. until it becomes a sticky paste, and then dry and grind to obtain doped ore powder; (3) Calcination: ammonium sulfate and the doped ore powder prepared in step (2) are mixed, spread on a crucible, placed in a tube furnace, and air is introduced. The temperature in the tube furnace is raised to 190-210° C. at a rate of 8-12° C. / min, kept at that temperature for 25-35 min, then raised to 390-410° C. at a rate of 4-6° C. / min, kept at that temperature for 100-140 min, and cooled to room temperature to obtain a calcined ore powder; (4) Leaching: adding the calcined powder prepared in step (3) into deionized water, heating to 65-75°C, stirring for 40-80 minutes, filtering at normal pressure to obtain a filtrate, which is the leachate; (5) impurity removal: add hydrogen peroxide to the leachate prepared in step (4), heat to 55-65°C, stir for 40-80 min, then adjust the pH to 4.9-5.1 with industrial ammonia water, let stand for 4-8 h, filter at normal pressure, take the filtrate, add sodium diethyldithiocarbamate trihydrate to the filtrate, heat to 60-80°C, stir for 20-40 min, let stand for 10-14 h, filter at normal pressure, then add ammonium fluoride, heat to 80-95°C, stir for 50-60 min, let stand for 10-14 h, filter at normal pressure to obtain a manganese-rich solution; (6) Manganese precipitation: adjust the pH of the manganese-rich solution prepared in step (5) to 9.8-10.5 using aqueous ammonia, raise the temperature to 55-65°C, stir for 50-70 minutes, let stand for 10-14 hours to precipitate manganese, filter under normal pressure, and dry the filter cake to obtain the manganese precipitate; (7) Oxidation: Add the manganese precipitate prepared in step (4) into deionized water, stir for 20-40 min, then add industrial ammonia water to adjust the pH value to 9.5-10.5, then add hydrazine hydrate, react for 7-9 h, filter, wash, and dry at 70-80 ° C for 3-5 h to obtain a trimanganese tetraoxide precursor; In the step (2), the weight ratio of high iron rhodochrosite powder, urea and thiourea is 1:0.18-0.22:0.04-0.

06.

2. The process for preparing a manganese tetraoxide precursor based on an ammonium sulfate system according to claim 1, characterized in that: The amount of ammonium sulfate added in step (3) is 1.7-1.9 times the weight of the high-iron rhodochrosite powder in the doped ore powder.

3. The process for preparing manganese tetraoxide precursor based on ammonium sulfate system according to claim 1, characterized in that: In step (3), the end of the tubular furnace is connected to a gas collecting bottle, and the liquid in the gas collecting bottle is a 1 mol / L sulfuric acid solution.

4. The process for preparing manganese tetraoxide precursor based on ammonium sulfate system according to claim 1, characterized in that: The air flow rate in step (3) is 0.8-1.2 L / min.

5. The process for preparing manganese tetraoxide precursor based on ammonium sulfate system according to claim 1, characterized in that: In step (5), the amount of hydrogen peroxide added to the leaching solution is 15-25 ml / L.

6. The process for preparing manganese tetraoxide precursor based on ammonium sulfate system according to claim 1, characterized in that: In the step (5), the amount of sodium diethyldithiocarbamate trihydrate added to the leaching solution is 0.13-0.16 g / L.

7. The process for preparing manganese tetraoxide precursor based on ammonium sulfate system according to claim 1, characterized in that: In the step (5), the amount of ammonium fluoride added to the leaching solution is 4-4.5 g / L.

Citation Information

Patent Citations

  • Preparation method for manganic manganous oxide

    CN105417586A

  • Method for preparing trimanganese tetroxide by utilizing acid-soluble manganese ore and on basis of sulfur-ammonia circulation

    CN107381646A

  • Method for preparing high-purity manganese sulfate by reducing and leaching pyrolusite from rotary kiln slag

    CN112777642A

  • Method for producing manganese sulfate from by-products of zinc smelting process

    KR102612151B1

  • Method for recycling multiple valuable metals from lateritic nickel ore and regeneration cycle of acid-alkaline double medium

    WO2022036775A1

Cited By

  • Manganese tetraoxide for lithium ion battery and preparation method thereof

    CN120887455A

  • Method for recovering manganese from low-grade manganese carbonate ore at low temperature

    CN120945191A

  • A method for recovering manganese from low-grade manganese carbonate ores at low temperatures

    CN120945191B

  • Method for recovering manganese from manganese-iron alloy waste residues

    CN120945233A

  • A method for recovering manganese from ferromanganese alloy waste residues

    CN120945233B