Preparation of 1-(2-alkoxy ethyl) piperidine regulator and regulation of 1-(2-alkoxy ethyl) piperidine regulator on poly-conjugated diene side group structure
By using 1-(2-alkoxyethyl)piperidine as anionic polymerization regulator, the problem that the regulator in the prior art is difficult to meet multiple requirements at high temperatures is solved, and rapid polymerization rate and efficient side group structure regulation are achieved. , a polymer with a high pendant content was prepared.
Patent Information
- Application Number
- CN202411102720.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-12
AI Technical Summary
At high temperature, the existing anionic polymerization regulators are difficult to meet the requirements of low dosage, strong regulation ability, fast polymerization rate and less affected by the structure adjustment ability, which makes it difficult to prepare polymerization with high side group content in industrial production. Things.
1-(2-alkoxyethyl)piperidine is used as anionic polymerization regulator, and prepared by condensation reaction, and butadiene, isoprene, and styrene monomer are added to the anionic polymerization, and organic lithium is used as the initiator. The agent is polymerized at a temperature of 0°C to 100°C to obtain a homopolymer or copolymer with a high pendant group content.
The rapid polymerization rate and efficient regulation of the side group structure at higher temperatures are achieved. The molecular weight of the polymer can be designed, the molecular weight distribution is narrow, and the glass transition temperature can be adjusted to obtain a polymer with a high side group content.
Smart Images

Figure CN118994058A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for preparing 1-(2-alkoxyethyl)piperidine and an anionic polymerization regulator system containing 1-(2-alkoxyethyl)piperidine. Under the regulator system, the obtained butadiene, isoprene and copolymers thereof with styrene all have high side group content, especially in polybutadiene, the vinyl content can reach up to 92%, which is manifested as a higher glass transition temperature, T g =4.06℃. Background Art
[0002] With the rapid development of the aerospace and automotive industries, it is very important to develop new elastomeric materials with special uses and energy conservation and environmental protection. The conjugated diene homopolymer with high side group structure has high anti-skid properties, low rolling resistance and thermal oxidation aging resistance, and is an ideal high-performance green tire rubber; in addition, the random copolymer structure of butadiene, isoprene and styrene with medium and high side group structure can also reduce rolling resistance and improve rebound.
[0003] Anionic polymerization has unique advantages over coordination polymerization in the preparation of the above-mentioned rubbers, including: (1) Anionic polymerization products have methodological advantages in functionalization and topological structure design. Coordination polymerization is more difficult to operate, and the number of functionalized free chain ends is often uncontrollable. In addition, anionic polymerization can introduce heteroatoms at the ends of polymer molecular chains through initiators or end capping from the perspective of molecular design, which significantly reduces the number of free ends and theoretically reduces heat generation more significantly. (2) The components of the lithium initiator system are relatively simple, and the post-treatment in the production process is simple (compared with coordination polymerization products that do not require deashing), and the molecular weight is controllable; (3) It is easy to adjust the side group content and the adjustment range is wide, which can conveniently prepare polyconjugated diene rubber varieties with different side group contents; (4) The lithium initiator system has high activity, less initiator usage, high production efficiency, and less pollution from three wastes; (5) In addition to producing BR, the lithium-based polymerization equipment can also be used for the production of SSBR and styrene TPS (SBS / SIS and SEBS / SEPS products) after minor adjustments, and the production line can be flexibly changed according to the market.
[0004] In anionic polymerization, a structural regulator with strong regulating ability is selected for preparation. It is necessary to select a structural regulator with strong regulating ability and less affected by high temperature at the same dosage. At present, among the regulators for anionic polymerization, those with strong regulating ability include dipiperidylethane (DPE), tetramethylethylenediamine (TMEDA), pentamethyldiethylenetriamine (PMEDTA), tetrahydrofurfuryl alcohol ether (ETE), N,N-dimethyltetrahydrofurfurylamine (THF-EDA), ditetrahydrofurfuryl propane (DTP), etc. These regulators have some shortcomings.
[0005] Generally speaking, the side group content of the polymer prepared by using a regulator depends on the type and amount of the regulator used and the polymerization temperature. For example, if a higher polymerization temperature is used, the side group content of the obtained polymer will be reduced. US4247418 introduces several regulators with a bicyclic symmetrical structure such as bispiperidinylethane (DPE). This type of regulator can obtain polybutadiene with a side group structure close to 100% at 5-10°C, but at a polymerization temperature of 70°C, only 30.7% of the side group structure can be obtained under the ratio of DPE / Li=1.0. In addition, low-temperature polymerization has a long induction period and a slow polymerization rate, and is more harmful to the environment, which limits its industrial application.
[0006] Increasing the polymerization temperature usually speeds up the polymerization rate. Therefore, in industrial production, it is hoped that the polymerization reaction can be carried out at a moderately high temperature and the production volume can be maximized. However, the polymerization rate of some regulators decreases when the temperature increases. The most typical one is tetramethylethylenediamine (TMEDA). Halasa et al. demonstrated that in the homopolymerization of isoprene, the T g As the proportion of the regulator increases, the polymerization rate decreases with the increase of the polymerization temperature. In addition, T g The polymerization temperature has a significant influence on the polymerization. When the TMEDA / Li ratio is 2.0, the T g When the temperature drops from about -11°C to -28°C, the pendant group content decreases greatly (reference CC Chang, AF Halasa, and JW Miller, J. Appl. Polym. Sci. 47, 1589 (1993)).
[0007] In addition, most current regulators are difficult to prepare polymers with high side group content when the polymerization temperature is above 50°C and only a low regulator ratio is used. US5231153 reports a new type of structural regulator, alkyl tetrahydrofurfuryl ether. Taking ethyl tetrahydrofurfuryl ether (ETE) as a structural regulator, a polymer with a side group content of 76% and T g = 0℃ polyisoprene. Compared with 2G, TMEDA, etc., this type of regulator has the characteristics of "small dosage, strong regulating ability, and less influence of temperature on regulating ability", and its polymerization rate is positively correlated with polymerization temperature. However, this type of regulator is easy to saturate, and the peak value of side group content is only about 75%.
[0008] In summary, it is currently difficult for a single regulator to simultaneously meet the following requirements:
[0009] (1) Small amount of regulator: At a polymerization temperature above 50°C, only a relatively low amount of regulator can be used to obtain a homopolymer with more than 70% side group structure.
[0010] (2) Strong regulating ability of the regulator: At a polymerization temperature above 50°C, it has a strong structural regulating ability, with a peak value greater than 82%, and can be used to prepare polyconjugated dienes with ultra-high side group structures.
[0011] (3) The polymerization rate is fast and the regulator ratio is positively correlated with the polymerization rate.
[0012] (4) Within a certain temperature range, the structural regulation ability is less affected by the polymerization temperature. Summary of the invention
[0013] In order to overcome the above problems of existing regulators, the present invention relates to a 1-(2-alkoxyethyl)piperidine regulator (Formula I) and a preparation method, and an anionic polymerization regulator system containing 1-(2-alkoxyethyl)piperidine shown in (Formula I).
[0014] According to the first aspect of the present invention, the present invention provides a 1-(2-alkoxyethyl)piperidine modulator having a structure shown in (Formula I):
[0015]
[0016] Wherein, R is a C1-C6 alkyl group.
[0017] According to the first aspect of the present invention, the present invention provides a method for preparing 1-(2-alkoxyethyl)piperidine, characterized in that the preparation method comprises: using 1-(2-hydroxyethyl)piperidine (Formula II) as a raw material, and under alkaline conditions, 1-(2-hydroxyethyl)piperidine and a haloalkane RX undergo a condensation reaction to obtain the obtained product, and the chemical reaction formula is shown in (Formula III).
[0018]
[0019] Wherein, R is a C1-C6 alkyl group.
[0020] The amounts of the potassium hydroxide, the alkyl halide RX and the 1-(2-hydroxyethyl)piperidine are reasonably selected according to actual conditions. For example, the molar ratio of the 1-(2-hydroxyethyl)piperidine, potassium hydroxide and the alkyl halide can be 1:1.0-4.0:1.0-6.0, preferably 1:1.0-2.0:1.0-3.0.
[0021] According to the second aspect of the present invention, the present invention provides a method for regulating the side group structure of a polyconjugated diene: in anionic polymerization, a regulator (1-(2-alkoxyethyl) piperidine) is added to a non-polar hydrocarbon solvent, and then one or two of butadiene, isoprene, and styrene (St) monomers are added, and organic lithium is used as an initiator. Polymerization is carried out at a temperature of 0°C to 100°C for 0.1 to 5.0 hours to obtain a homopolymer or a binary copolymer having a content of 1,2-structure and 3,4-structure of ≥70%;
[0022] The -R group of 1-(2-alkoxyethyl)piperidine (Formula I) used in the present invention includes but is not limited to ethyl, propyl, butyl, isopropyl, isobutyl, and cyclohexyl, and is particularly preferably ethyl, propyl, and butyl.
[0023] The regulator system composed of 1-(2-alkoxyethyl)piperidine in the present invention is characterized in that the molar ratio of the regulator to the organic lithium initiator is in the range of 0.1 to 10.0, preferably in the range of 0.5 to 5.0.
[0024] The active center of the organic lithium compound used in the present invention can be any one of monolithium, dilithium or polylithium initiators, and the organic lithium compound is selected from one or a combination of alkyl lithium, aryl lithium, functional lithium, organic lithium chloride, and macromolecular active lithium. The alkyl lithium is n-butyl lithium, sec-butyl lithium, tert-butyl lithium, methyl lithium, diphenylhexyl lithium, etc.; the functional lithium is dimethylamine lithium, diethylamine lithium, diisopropylamine lithium, cyclohexylimide lithium, piperidyl lithium, etc.; the organic lithium chloride is n-butyl lithium chloride, isobutyl lithium chloride; the macromolecular active lithium is polystyrene active lithium, polybutadiene active lithium, polyisoprene active lithium or poly-1,3-hexadiene active lithium. Preferably, it is n-butyl lithium, sec-butyl lithium, tert-butyl lithium, polystyrene active lithium, and polybutadiene active lithium.
[0025] The polymerizable monomers in the present invention may be styrene and its derivatives and conjugated dienes, wherein styrene and its derivatives may be one or more of styrene, vinyl toluene, α-methyl styrene, 4-tert-butyl styrene and 4-methyl styrene; the conjugated dienes may be one or more of butadiene, isoprene, piperylene, 1,3-hexadiene and 2,3-dimethylbutadiene. From the perspective of raw material availability and market demand, butadiene, isoprene and styrene are particularly preferred.
[0026] The non-polar organic solvent used in the present invention includes, but is not limited to, cyclohexane, n-hexane, n-pentane, n-heptane, toluene, benzene, or one or a combination of hydrogenated oil or extracted oil, preferably cyclohexane.
[0027] In the mixed solution of the conjugated diene and the non-polar hydrocarbon solvent used in the present invention, the monomer mass concentration of the conjugated diene is in the range of 5% to 20%, preferably 8% to 15%.
[0028] The terminator used in the present invention includes but is not limited to any one of water, methanol, ethanol, and isopropanol, preferably isopropanol.
[0029] According to the regulator system composed of 1-(2-alkoxyethyl)piperidine in the present invention, it is characterized in that the microstructure of the prepared polymer is controllable and can obtain a higher side group content. For butadiene monomer, in its homopolymer microstructure, the side group content of the butadiene unit ranges from 50% to 95%, preferably from 70% to 95%; for isoprene monomer, in its homopolymer microstructure, the side group content of the isoprene unit ranges from 50% to 95%; in the microstructure of butadiene and styrene copolymers, the side group content of the butadiene unit ranges from 50% to 90%, preferably from 70% to 90%; preferably from 70% to 95%. In the microstructure of isoprene and styrene copolymers, the side group content of the isoprene unit ranges from 50% to 90%, preferably from 70% to 90%.
[0030] According to the polymer prepared by the regulator system composed of 1-(2-alkoxyethyl)piperidine in the present invention, its M n The range is 1×10 3 ~5×10 5 g / mol, preferably 2×10 4 ~2×10 5 g / mol, the distribution width PDI value of the polymer is between 1.0 and 1.5, preferably in the range of 1.0 to 1.2.
[0031] The polymer prepared by the regulator system composed of 1-(2-alkoxyethyl)piperidine in the present invention has a controllable glass transition temperature range and has a higher T value due to the ability to obtain a higher content of side group structures. g For example: PB's T g The range is between -60℃ and 5℃, and the preferred range is -40℃ to 5℃. g The range is between -40℃ and 20℃, and the preferred range is -20℃ to 15℃.
[0032] The beneficial effects of the present invention are:
[0033] The 1-(2-alkoxyethyl)piperidine regulator is synthesized in one step through a condensation reaction with a high yield.
[0034] 1-(2-alkoxyethyl)piperidine is used as a regulator for anionic polymerization in the homopolymerization of butadiene and isoprene and its copolymerization with styrene. The reaction activity is controllable, the monomer conversion is basically complete, the molecular weight of the polymer can be designed in a wide range, and the number average molecular weight M n In 1×10 3 ~5×10 5 g / mol, and the molecular weight distribution is narrow, ranging from 1.02 to 1.08. Compared with other regulators, its advantages are:
[0035] 1. The polymerization rate is fast, and the polymerization rate increases with the increase of the regulator ratio. For example, when 1.0 equivalent of regulator is used, the conversion rate of butadiene monomer reaches more than 90% within 0.5h at 50°C;
[0036] 2. At higher polymerization temperatures, the regulator still exhibits efficient regulation of the 1,2- / 3,4-structure. For example, at 50°C, only 0.5 equivalents of the regulator are needed to obtain polybutadiene with a high 1,2-structure content (72.68%).
[0037] 3. In addition, at higher temperatures, the regulator still exhibits a strong ability to regulate the 1,2- / 3,4-structure. For example, at 70°C, in butadiene polymerization, using 5.0 equivalents of the regulator, polybutadiene with an ultra-high 1,2-structure (85.80%) was obtained;
[0038] 4. Finally, under the action of the regulator, butadiene and isoprene also show good randomness during the copolymerization process with styrene.
[0039] The present invention will be described in detail below through examples. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 The 1-(2-alkoxyethyl)piperidine modifier of Preparation Examples 1 to 7 is 13 C NMR spectrum.
[0041] Figure 2 is the polybutadiene of Example 1 1 H NMR spectrum.
[0042] Figure 3 is the polybutadiene of Example 1 13 C NMR spectrum.
[0043] Figure 4 This is a DSC curve chart of the polybutadiene of Example 1.
[0044] Figure 5 It is a kinetic curve diagram of the polybutadiene of Examples 1 and 12 to 14 at different EtOEP / Li ratios.
[0045] Figure 6 is the polyisoprene of Example 18 1 H NMR spectrum.
[0046] Figure 7 It is a kinetic curve diagram of the polyisoprene of Examples 17 to 20 at different EtOEP / Li ratios.
[0047] Figure 8 is the butadiene-styrene random copolymer of Example 24 1 H NMR spectrum.
[0048] Fig. 9 is a DSC curve chart of the butadiene-styrene block copolymer of Example 35. DETAILED DESCRIPTION
[0049] The present invention is illustrated by the following examples, which are not intended to limit the scope or implementation of the present invention.
[0050] In the following examples, the molecular structure of organic matter and the microstructure content of polymer were determined by nuclear magnetic resonance spectrometer (NMR), the composition and content of organic matter were determined by gas chromatograph (GC), and the glass transition temperature T of polymer was determined by differential scanning calorimeter (DSC). g The number average molecular weight and weight average molecular weight of the polymer (THF as mobile phase) were determined by gel permeation chromatography (GPC). The Mooney viscosity of the raw rubber of the polymer was determined by Mooney viscosity tester.
[0051] Preparation Example 1
[0052] This preparation example is used to illustrate the preparation method of 1-(2-alkoxyethyl)piperidine provided by the present invention.
[0053] 0.15 mol of 1-(2-hydroxyethyl)piperidine, 0.3 mol of potassium hydroxide and 0.45 mol of ethyl bromide were added to a single-necked flask, covered with a condenser, and refluxed at 50°C for 12 hours. Poured into a separatory funnel, extracted with ether three times, the organic layer was dried over anhydrous magnesium sulfate, and the fractions were collected by vacuum distillation to obtain 99.56% of 1-(2-ethoxyethyl)piperidine (EtOEP, 1-(2-ethoxyethyl)piperidine), with a yield of 87%.
[0054] Preparation Example 2
[0055] This preparation example is used to illustrate the preparation method of 1-(2-alkoxyethyl)piperidine provided by the present invention.
[0056] 0.15 mol of 1-(2-hydroxyethyl)piperidine, 0.25 mol of potassium hydroxide and 0.45 mol of ethyl bromide were added to a single-necked flask, covered with a condenser, and refluxed at 50°C for 12 hours. Poured into a separatory funnel, extracted with ether three times, dried the organic layer with anhydrous magnesium sulfate, and then distilled under reduced pressure to collect the fractions. The yield of EtOEP was 84%.
[0057] Preparation Example 3
[0058] This preparation example is used to illustrate the preparation method of 1-(2-alkoxyethyl)piperidine provided by the present invention.
[0059] 0.15 mol of 1-(2-hydroxyethyl)piperidine, 0.25 mol of potassium hydroxide and 0.4 mol of ethyl bromide were added to a single-necked flask, covered with a condenser, and refluxed at 40°C for 18 hours. Poured into a separatory funnel, extracted with ether three times, the organic layer was dried over anhydrous magnesium sulfate, and the fractions were collected by vacuum distillation. The yield of EtOEP was 82%.
[0060] Preparation Example 4
[0061] 1-(2-alkoxyethyl)piperidine was prepared according to the method of Preparation Example 1, except that the ethyl bromide was replaced by the same mole of n-propane bromide to obtain 99.23% of 1-(2-propoxyethyl)piperidine (n-PrOEP, 1-(2-propoxyethyl)piperidine) with a yield of 79%.
[0062] Preparation Example 5
[0063] 1-(2-alkoxyethyl)piperidine was prepared according to the method of Preparation Example 1, except that the bromoethane was replaced by the same mole of 2-bromopropane to obtain 98.12% of 1-(2-isopropoxyethyl)piperidine (i-PrOEP, 1-(2-isopropoxyethyl)piperidine) with a yield of 47%.
[0064] Preparation Example 6
[0065] 1-(2-alkoxyethyl)piperidine was prepared according to the method of Preparation Example 1, except that the bromoethane was replaced by n-bromobutyl with the same molar number of moles, to obtain 99.44% of 1-(2-butoxyethyl)piperidine (n-BuOEP, 1-(2-butoxyethyl)piperidine) with a yield of 95%.
[0066] Preparation Example 7
[0067] 1-(2-alkoxyethyl)piperidine was prepared according to the method of Preparation Example 1, except that the bromoethane was replaced by the same mole of isobutane bromide to obtain 99.17% of 1-(2-isobutoxyethyl)piperidine (i-BuOEP, 1-(2-isobutoxyethyl)piperidine) with a yield of 63%.
[0068] Figure 1 All regulators 13 C NMR spectrum.
[0069] Example 1
[0070] This example is used to illustrate the preparation method of a polymer having a high content of side group structures by anionic polymerization provided by the present invention.
[0071] In this experiment, polybutadiene with high 1,2-structure was synthesized using EtOEP as a regulator. In the procedure used, a cyclohexane solution of butadiene with a monomer mass concentration of 15%, EtOEP with a regulator / Li molar ratio of 1.0, and n-butyl lithium (n-BuLi) were added to a clean and impurity-free reactor in sequence, and the reaction was carried out at 50°C for 1 hour. After the polymerization reaction was completed, isopropanol (containing 1 phm of antioxidant) was added to terminate the reaction, and then methanol was used for precipitation. The resulting polymer was dried in a vacuum oven at 50°C until the mass was constant. The prepared polybutadiene had a glass transition temperature (T) of -23.71°C as determined by DSC. g ).pass 1 H NMR analysis showed that the polymer contained 81.57% 1,2-PB and 18.43% 1,4-PB. Figure 2 It is polybutadiene 1 HNMR spectrum, Figure 3 It is polybutadiene 13 C NMR spectrum, Figure 4 It is the DSC curve of polybutadiene.
[0072] Example 2
[0073] In this example the procedure described in Example 1 was used except that n-PrOEP was used as the modulator. 1 H NMR determined that it contained 77.19% 1,2-PB and 22.81% 1,4-PB.
[0074] Example 3
[0075] In this example the procedure described in Example 1 was used except that i-PrOEP was used as the modulator. 1 H NMR determined that it contained 78.88% 1,2-PB and 21.12% 1,4-PB.
[0076] Example 4
[0077] In this example the procedure described in Example 1 was used except that n-BuOEP was used as the modifier. The polybutadiene produced was determined to have a T of -24.85°C. g .pass 1 H NMR determined that it contained 81.12% 1,2-PB and 18.88% 1,4-PB.
[0078] Example 5
[0079] In this example the procedure described in Example 1 was used except that i-PrOEP was used as the modulator. 1 H NMR determined that it contained 76.78% 1,2-PB and 23.22% 1,4-PB. The T g The microstructures are listed in Table 1.
[0080] Table 1. Examples 1 to 5
[0081]
[0082] Embodiments 6 to 11
[0083] The procedure described in Example 1 was used in these examples, except that the polymerization was carried out at different temperatures and the EtOEP / n-BuLi ratio was adjusted from 0.5 to 5.0. The T g The microstructures are listed in Table 2.
[0084] Table 2. Examples 6 to 11
[0085]
[0086] Embodiments 12 to 16
[0087] In this example, the procedure described in Example 1 was used, except that the amount of EtOEP was changed, and the EtOEP / BuLi ratio was changed from 1.0 to 0.5-20.0. The T of the obtained polybutadiene g The microstructures are listed in Table 3. Figure 5 It is the kinetic curve diagram of different regulator ratios.
[0088] Table 3. Examples 12 to 16
[0089]
[0090] Examples 17 to 22
[0091] In these examples, the procedure described in Example 1 was used, except that isoprene was used as the polymerization monomer and the EtOEP / n-BuLi ratio was adjusted from 0.5 to 20.0. The T of the resulting polyisoprene g The microstructures are listed in Table 4. Figure 6 It is polyisoprene 1 H NMR spectrum, Figure 7 It is the kinetic curve diagram of different regulator ratios.
[0092] Table 4. Examples 17 to 22
[0093]
[0094] Embodiments 23 to 28
[0095] The procedure described in Example 1 was used in these examples, except that styrene / butadiene with a weight ratio of 20 / 80 was used as the polymerization monomers, and the EtOEP / n-BuLi ratio was adjusted from 0.5 to 20.0. The T of the obtained styrene-butadiene copolymers g The microstructures are listed in Table 5. 1 H NMR confirmed that it has a high vinyl structure, a low block styrene content, and a good degree of styrene randomization. Figure 8 Butadiene-styrene copolymer 1 H NMR spectrum.
[0096] Table 5. Examples 23 to 28
[0097]
[0098] Examples 29 to 34
[0099] The procedure described in Example 1 was used in these examples except that styrene / isoprene with a weight ratio of 20 / 80 was used as the polymerization monomers and the EtOEP / n-BuLi ratio was adjusted from 0.5 to 20.0. The T g The EtOEP / n-BuLi ratios used are listed in Table 6.
[0100] Table 6. Examples 29 to 34
[0101]
[0102] Embodiment 35
[0103] In this experiment, SBS with high 1,2-structure (styrene mass fraction of 20%) was synthesized using piperidinyl ethyl ether as a regulator. In the procedure used, 2.5L cyclohexane was added to a 5L reactor that had been cleaned and impurities removed, and then 64mL styrene, 1.80mL pure piperidinyl ethyl ether and 7.4ml of 0.50M sec-butyl lithium solution were added to the reactor by syringe to initiate polymerization (the molar ratio of regulator / butyl lithium was 2.5). After 0.5 hours at 50°C, 376mL butadiene was added and the reaction continued for 1 hour. SiCl4 was added at a rate of 3.5 arms for coupling. After half an hour of reaction, the glue solution was released and ethanol was added to terminate the reaction. 1phm of antioxidant was added. After evaporating the cyclohexane, the water was dried by mixing with an open mill, and the resulting polymer was dried in a vacuum oven at 50°C to obtain 290g of dry glue. Fig. 9 The DSC curve of SBS shows two glass transition temperatures (T) at -34.75°C and 75.07°C. g ).pass 1 H NMR determined that it had a microstructure containing 74% 1,2-polybutadiene units and 26% 1,4-polybutadiene units. GPC determined that the component contained 88% SBS, 10% SB, and 2% PS.
Claims
1. Preparation of 1-(2-alkoxyethyl)piperidine regulator and its regulation of the side group structure of polyconjugated diene, characterized in that The structure of the 1-(2-alkoxyethyl)piperidine modulator is shown in Formula I: Wherein, R is a C1-C6 alkyl group.
2. The preparation method of 1-(2-alkoxyethyl)piperidine is characterized in that The preparation method comprises: using 1-(2-hydroxyethyl)piperidine (Formula II) as a raw material, and carrying out a condensation reaction between 1-(2-hydroxyethyl)piperidine and a haloalkane RX under alkaline conditions to obtain the obtained product, and the chemical reaction formula is shown in (Formula III). Wherein, R is a C1-C6 alkyl group. The amounts of the potassium hydroxide, the alkyl halide RX and the 1-(2-hydroxyethyl)piperidine are reasonably selected according to actual conditions. For example, the molar ratio of the 1-(2-hydroxyethyl)piperidine, potassium hydroxide and the alkyl halide can be 1:1.0-4.0:1.0-6.0, preferably 1:1.0-2.0:1.0-3.
0.
3. Preparation of 1-(2-alkoxyethyl)piperidine regulator and its regulation of the side group structure of polyconjugated diene, characterized in that The method for adjusting the side group structure of polyconjugated diene is as follows: in anionic polymerization, a regulator (1-(2-alkoxyethyl) piperidine) is added to a non-polar hydrocarbon solvent, and then one or two of butadiene, isoprene, and styrene (St) monomers are added, and organic lithium is used as an initiator. The polymerization is carried out at a temperature of 0°C to 100°C for 0.1 to 5.0 hours to obtain a homopolymer or a binary copolymer with a content of 1,2-structure and 3,4-structure of ≥70%.
4. Preparation of 1-(2-alkoxyethyl)piperidine regulator and its regulation of the side group structure of polyconjugated diene, as described in claim 1, characterized in that: The -R group in 1-(2-alkoxyethyl)piperidine is selected from ethyl, propyl, butyl, isopropyl, isobutyl and cyclohexyl.
5. As claimed in claim 3, a regulator system consisting of 1-(2-alkoxyethyl)piperidine is used, characterized in that The molar ratio of the regulator to the organic lithium initiator is in the range of 0.1 to 10.0, preferably in the range of 0.5 to 5.
0.
6. As claimed in claim 3, a regulator system consisting of 1-(2-alkoxyethyl)piperidine is used, characterized in that The active center of the organic lithium compound can be a monolithium, dilithium or polylithium initiator, and the organic lithium compound is selected from one or a combination of alkyl lithium, aryl lithium, functional lithium, organic lithium chloride, and macromolecular active lithium, and the organic lithium is preferably an alkyl lithium.
7. As claimed in claim 3, a regulator system consisting of 1-(2-alkoxyethyl)piperidine is used, characterized in that The non-polar organic solvent is selected from one or a combination of cyclohexane, n-hexane, n-pentane, n-heptane, toluene, benzene, hydrogenated oil or extracted oil, and preferably the non-polar organic solvent is cyclohexane.
8. According to claim 3, a regulator system consisting of 1-(2-alkoxyethyl)piperidine is used, characterized in that: The microstructure of the prepared polymer can be controlled and a higher side group content can be obtained. For butadiene monomer, in its homopolymer microstructure, the side group content of the butadiene unit ranges from 50% to 95%, preferably from 70% to 95%; for isoprene monomer, in its homopolymer microstructure, the side group content of the isoprene unit ranges from 50% to 95%; in the microstructure of butadiene and styrene copolymers, the side group content of the butadiene unit ranges from 50% to 90%, preferably from 70% to 90%; preferably from 70% to 95%. In the microstructure of isoprene and styrene copolymers, the side group content of the isoprene unit ranges from 50% to 90%, preferably from 70% to 90%.
9. As claimed in claim 3, characterized in that The M of the prepared polymer n The range is 1×10 3 ~5×10 5 , preferably 2×10 4 ~2×10 5 The distribution width PDI value of the polymer is between 1.0 and 1.5, and the preferred range is between 1.0 and 1.
2.
10. As claimed in claim 3, characterized in that The glass transition temperature (T g ) ranges from -60°C to 5°C, preferably from -40°C to 5°C. The T of polyisoprene (PI) g The range is between -40℃ and 20℃, and the preferred range is -20℃ to 15℃.
Citation Information
Patent Citations
Terpolymer rubber with medium / high side group content and preparation method and applications thereof
CN102372823A
Structure adjusting agent for olefin anionic polymerization, ternary copolymerized rubber, preparation method and application thereof
CN104059196A
Regulator and method for controlling microstructure of butadiene homopolymer and copolymer
CN1844169A
Synthesis of random styrene-isoprene rubbers
US5173550A