Self-extinction acrylic dispersion, preparation method thereof and coating
The self-massed acrylic dispersion is prepared through polymer polymerization technology, which solves the problems of poor compatibility of matting additives and insufficient polymerization stability in the coating, achieves high permeability and stability of the paint film, and improves the appearance of the paint film and performance.
Patent Information
- Application Number
- CN202411108971.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-22
AI Technical Summary
The additional matting additives added to existing coatings are poorly compatible with the resin, resulting in poor permeability and insufficient stability of the paint film. The macromolecular gels or particles prepared by emulsion polymerization are prone to settlement and residue problems, which affects the resistance of the paint film. and appearance.
The self-massed acrylic dispersion is prepared by polymer polymerization technology. By adding mixed monomers and neutralizing agents to the suspension containing PMMA microspheres, the insulation reaction and dispersion are carried out to form a self-emulsified hydrophilic structure of a self-emulsified acrylic dispersion. Ensure the glass transition temperature and particle size distribution of PMMA microspheres, and improve compatibility and stability.
It achieves excellent extinction effect of the paint film, improves permeability and stability, avoids graying and mists in the paint film, and enhances the adhesion, hardness and aging resistance of the paint film.
Smart Images

Figure CN118994466A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of coating raw materials, in particular to a self-matting acrylic acid dispersion and a preparation method thereof, and a coating. Background Art
[0002] With the development of the coating industry, in order to obtain a paint film with a matte effect, the main measure currently adopted is to add an additional matte aid when preparing the paint sample. There is also a sol-gel technology that hydrolyzes and condenses organic siloxanes with functional groups under certain conditions and then grafts them into the chain segments of acrylic emulsions. The latex particles have bimodal or multimodal characteristics in particle size distribution, and express self-matting effects in the final paint film. In addition, there is also a method of using triethylamine as a catalyst, and first reacting amino silicone oil, polymer diol, diisocyanate, carboxylic acid diol, and small molecule diol to obtain a hydrophilic organic silicone modified polyurethane prepolymer, then adding a mixed diamine and water, stirring and emulsifying, and finally adding hexamethylene diisocyanate trimer, stirring and reacting to obtain organic silicone modified self-matting waterborne polyurethane for synthetic leather.
[0003] However, current technologies have the following disadvantages:
[0004] (1) The compatibility of the additionally added matting agent with the resin is relatively poor, resulting in poor permeability of the paint film, fogging on the surface of the paint film, unsatisfactory appearance, and affecting the durability of the paint film.
[0005] (2) The macromolecular gel or particles prepared by emulsion polymerization can achieve the effect of self-matting by forming concave and convex patterns on the surface of the paint film. However, while achieving self-matting with the help of incompatible particles and gels, stability problems are also prone to occur. In addition, the emulsifier added outside the emulsion polymerization will remain in the paint film, which will eventually affect the durability. The large-sized particles made by external emulsion polymerization have insufficient mechanical stability, cannot be ground and dispersed, and have poor fullness.
[0006] (3) By adding a polyurea structure to the polyurethane resin, storage problems such as sedimentation are less likely to occur, but the viscosity is likely to increase after hot storage, and due to the presence of a large number of hydrogen bonds, the solid content is low and the fullness is poor.
[0007] In view of this, the present invention is proposed. Summary of the invention
[0008] One object of the present invention is to provide a method for preparing a self-matting acrylic dispersion. The prepared self-matting acrylic dispersion has a good matting effect, ensures the permeability of the paint film, and has good stability.
[0009] Another object of the present invention is to provide a self-matting acrylic dispersion prepared by the above method.
[0010] Another object of the present invention is to provide a coating comprising the self-matting acrylic dispersion.
[0011] In order to achieve the above-mentioned object of the present invention, the present invention provides a method for preparing a self-matting acrylic dispersion, comprising the following steps:
[0012] (a) adding a first mixed monomer to a suspension containing PMMA microspheres and then incubating the mixture for reaction, and then adding a second mixed monomer and then incubating the mixture for reaction;
[0013] (b) adding a neutralizing agent to the system obtained in step (a) to carry out a neutralization reaction, and then adding water to disperse the system to obtain the self-matting acrylic dispersion;
[0014] The PMMA microsphere-containing suspension is mainly prepared from methyl methacrylate, a cross-linking monomer, a solvent, an initiator and an optional copolymer monomer; the glass transition temperature of the PMMA microsphere is ≥90° C., and the average particle size D50 of the PMMA microsphere is 5 to 15 μm.
[0015] In a specific embodiment of the present invention, in the preparation of the suspension containing PMMA microspheres, the mass ratio of the methyl methacrylate to the crosslinking monomer is 1:(0.1-0.5). Further, the crosslinking monomer includes at least one of trimethylolpropane trimethacrylate and 1,6-hexanediol diacrylate.
[0016] In a specific embodiment of the present invention, the comonomer includes at least one of styrene, cyclohexyl methacrylate, butyl methacrylate, isobornyl methacrylate, butyl acrylate, isooctyl acrylate, hydroxyethyl methacrylate, hydroxyethyl acrylate, hydroxypropyl methacrylate, propyl acrylate and methacrylic acid. Further, the mass of the comonomer is 0% to 40% of the mass of the methyl methacrylate.
[0017] In a specific embodiment of the present invention, the particle size of the PMMA microspheres satisfies at least one of the following characteristics:
[0018] (1) D10 is 3 to 7 μm;
[0019] (2) D90 is 15 to 25 μm.
[0020] In a specific embodiment of the present invention, the particle size distribution of the PMMA microspheres is approximately normal distribution.
[0021] In a specific embodiment of the present invention, the first mixed monomer includes any one or more of an acrylate monomer, a hydroxyl-containing acrylate monomer and a vinyl monomer, and a first initiator. Further, the first mixed monomer does not include a copolymerizable monomer containing a carboxyl group.
[0022] In a specific embodiment of the present invention, the second mixed monomer includes acrylic monomers, acrylate monomers, hydroxyl-containing acrylate monomers and a second initiator.
[0023] In a specific embodiment of the present invention, in step (a), the ratio of the sum of the mass of the first mixed monomer and the second mixed monomer to the mass of the PMMA microspheres is 1:(0.2-1).
[0024] In a specific embodiment of the present invention, the neutralizing agent includes at least one of triethylamine, triethanolamine and N,N-dimethylethanolamine.
[0025] Another aspect of the present invention provides a self-matting acrylic dispersion prepared by any one of the above-mentioned methods for preparing the self-matting acrylic dispersion.
[0026] In a specific embodiment of the present invention, the solid content of the self-matting acrylic dispersion is ≥45%, such as 45% to 48%.
[0027] Another aspect of the present invention provides a coating comprising any one of the self-matting acrylic dispersions described above.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] (1) The present invention adopts polymer polymerization technology to synthesize a self-matting acrylic dispersion. The PMMA microspheres can be well dispersed in the acrylic dispersion. When preparing the paint film, they can be suspended on the surface of the paint film to achieve an excellent matting effect. The problem of the paint film turning white and foggy due to the conventional addition of matting agents can be solved, and the permeability of the paint film can be improved.
[0030] (2) The self-matting acrylic dispersion of the present invention is a self-emulsifying hydrophilic structure and does not require the addition of an additional emulsifier, so the stability is greatly improved compared to the emulsion polymerization system. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0032] Figure 1 Schematic diagram of the self-matting acrylic dispersion provided in an embodiment of the present invention achieving the self-matting effect. DETAILED DESCRIPTION
[0033] The technical scheme of the present invention will be clearly and completely described below in conjunction with the accompanying drawings and specific embodiments, but it will be understood by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0034] In one aspect, the present invention provides a method for preparing a self-matting acrylic dispersion, comprising the following steps:
[0035] (a) adding a first mixed monomer to a suspension containing PMMA microspheres and then incubating the mixture for reaction, and then adding a second mixed monomer and then incubating the mixture for reaction;
[0036] (b) adding a neutralizing agent to the system obtained in step (a) to carry out a neutralization reaction, and then adding water to disperse the system to obtain a self-matting acrylic dispersion;
[0037] The suspension containing PMMA microspheres is mainly prepared from methyl methacrylate, a cross-linking monomer, a solvent, an initiator and an optional copolymer monomer; the glass transition temperature of the PMMA microspheres is ≥90°C, and the average particle size D50 of the PMMA microspheres is 5-15 μm.
[0038] Figure 1 A schematic diagram of the self-matting acrylic dispersion provided in an embodiment of the present invention to achieve the self-matting effect. In the self-matting acrylic dispersion of the present invention, PMMA microspheres are distributed in the acrylic dispersion resin in a granular state, and some of the PMMA microspheres are grafted to the resin to form a stable dispersion. After the dispersion is formed into a film and dried, the PMMA microspheres can achieve the surface roughness and microphase incompatibility of the paint film, thereby achieving the purpose of matting. Since the PMMA microspheres are partially bonded to the acrylic resin through chemical bonds and have similar structures to the acrylic resin, the compatibility of the self-matting acrylic dispersion is effectively improved, and the surface will not turn white and foggy after matting, and the paint film has good permeability and excellent stability.
[0039] In addition, the acrylic dispersion of the present invention is water-based and has excellent environmental protection compared to existing solvent-based acrylic resins. The acrylic dispersion of the present invention has a high solid content, excellent fullness, and the prepared paint film has good resistance.
[0040] The suspension containing PMMA microspheres of the present invention is obtained by solution polymerization. Methyl methacrylate, a cross-linking monomer, and an optional comonomer are polymerized under the action of an initiator to form PMMA microspheres, ensuring that the glass transition temperature of the PMMA microspheres is above 90°C, and ensuring that the PMMA microspheres will not deform under changing factors such as solvents and temperature, thereby affecting the matte effect. For example, in different embodiments, the glass transition temperature of the PMMA microspheres can be 90°C, 95°C, 98°C, 100°C, 105°C, 110°C, 120°C, etc., but is not limited thereto. Preferably, the glass transition temperature of the PMMA microspheres is ≥100°C.
[0041] The average particle size D50 of the PMMA microspheres of the present invention can be 5 μm, 6 μm, 8 μm, 10 μm, 12 μm, 14 μm, 15 μm or a range consisting of any two of them, so as to achieve both the matting effect and stability.
[0042] In a specific embodiment of the present invention, in the preparation of the suspension containing PMMA microspheres, the mass ratio of methyl methacrylate to the crosslinking monomer is 1:(0.1-0.5). Further, the crosslinking monomer includes at least one of trimethylolpropane trimethacrylate and 1,6-hexanediol diacrylate.
[0043] For example, in different embodiments, the mass ratio of methyl methacrylate to the crosslinking monomer can be 1:0.1, 1:0.2, 1:0.3, 1:0.4, 1:0.5 or any two of them. The ratio of the two is regulated within the above range to ensure that the glass transition temperature of the PMMA microspheres obtained meets the requirements.
[0044] In a specific embodiment of the present invention, the comonomer includes at least one of styrene cyclohexyl methacrylate, butyl methacrylate, isobornyl methacrylate, butyl acrylate, isooctyl acrylate, hydroxyethyl methacrylate, hydroxyethyl acrylate, hydroxypropyl methacrylate, propyl acrylate and methacrylic acid. Further, the mass of the comonomer is 0% to 40% of the mass of methyl methacrylate.
[0045] For example, in different embodiments, no comonomer may be added. If a comonomer is added, the mass of the comonomer may be 1%, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40% of the mass of methyl methacrylate or a range consisting of any two of them. The glass transition temperature of the PMMA microspheres formed can be adjusted by the amount of comonomer added, and the resistance can be regulated.
[0046] In a specific embodiment of the present invention, the particle size of the PMMA microspheres satisfies at least one of the following characteristics:
[0047] (1) D10 is 3 to 7 μm;
[0048] (2) D90 is 15 to 25 μm.
[0049] In a specific embodiment of the present invention, the particle size distribution of PMMA microspheres is approximately normal distribution.
[0050] The D10 particle size of the PMMA microspheres obtained can be 3 μm, 4 μm, 5 μm, 6 μm, 7 μm or a range consisting of any two thereof; the D90 particle size of the PMMA microspheres obtained can be 15 μm, 18 μm, 20 μm, 22 μm, 25 μm or a range consisting of any two thereof.
[0051] The particle size and distribution of the PMMA microspheres of the present invention can be adjusted by the dropping speed of the material during the preparation process. The faster the dropping speed, the larger the particle size of the corresponding PMMA microspheres and the larger the particle size distribution; the slower the dropping speed, the smaller the particle size of the corresponding PMMA microspheres and the smaller the particle size distribution. In the present invention, the preparation of the suspension containing PMMA microspheres includes: adding a mixed solution of methyl methacrylate, a cross-linking monomer, an initiator and an optional comonomer to a pre-heated solvent, and after the dropwise addition is completed, the reaction is kept warm. Among them, the dropping rate of the mixed solution can be controlled at 10 to 30 g / h, but is not limited thereto, and the specific dropping rate can be conventionally adjusted according to the particle size of the PMMA microspheres formed. The time of the insulation reaction can be 0.5 to 2 hours, such as 1 hour, etc. The temperature of the solvent preheating and the temperature of the insulation reaction can be adjusted according to the type of actual initiator to ensure the smooth progress of the solution polymerization, such as 100 to 120°C, but is not limited thereto.
[0052] In a specific embodiment of the present invention, in the preparation of the suspension containing PMMA microspheres, the solvent includes at least one of ethylene glycol butyl ether and propylene glycol butyl ether. Further, the mass of the solvent is 0.3 to 1.2 times the mass of methyl methacrylate.
[0053] For example, in different embodiments, the mass of the solvent may be 0.3 times, 0.5 times, 0.8 times, 1 times, 1.2 times, or a range consisting of any two of the mass of methyl methacrylate.
[0054] In a specific embodiment of the present invention, in the preparation of the suspension containing PMMA microspheres, the initiator includes BPO. Further, in the preparation of the suspension containing PMMA microspheres, the reaction temperature is 100-120°C.
[0055] In a specific embodiment of the present invention, the first mixed monomer includes any one or more of an acrylate monomer, a hydroxyl-containing acrylate monomer and a vinyl monomer, and a first initiator. Further, the first mixed monomer does not include a copolymerizable monomer containing a carboxyl group.
[0056] Among them, in the first mixed monomer, the acrylic ester monomer includes at least one of methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, cyclohexyl methacrylate, isobornyl methacrylate and lauric acrylate; the hydroxyl-containing acrylic ester monomer includes at least one of hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate and hydroxybutyl (meth)acrylate; and the vinyl monomer includes styrene. The amount of each specific monomer in the first mixed monomer can be adjusted according to the requirements of the acrylic dispersion.
[0057] In a specific embodiment of the present invention, in the first mixed monomer, the mass ratio of the acrylic ester monomer, the hydroxyl-containing acrylic ester monomer and the vinyl monomer can be (10-15): (3-6): (0-3).
[0058] For example, in different embodiments, the first mixed monomer may not contain vinyl monomers, and the mass ratio of acrylate monomers to hydroxyl-containing acrylate monomers may be 10:3, 10:4, 10:5, 10:6, 12:3, 12:4, 12:5, 15:3, 15:4, 15:6 or a range consisting of any two of them; when containing vinyl monomers, the mass ratio of acrylate monomers to vinyl monomers may be 10:1, 12:1, 15:1, 10:2, 12:2, 15:2, 10:3, 12:3, 15:3 or a range consisting of any two of them.
[0059] In a specific embodiment of the present invention, in the first mixed monomer, the first initiator includes a peroxide initiator, such as at least one of tert-butyl perbenzoate, di-tert-butyl hydroperoxide, and di-tert-amyl peroxide. The amount of the first initiator can be 0.1% to 1.5% of the mass of each monomer in the first mixed monomer, but is not limited thereto.
[0060] In a specific embodiment of the present invention, the second mixed monomer includes acrylic monomers, acrylate monomers, hydroxyl-containing acrylate monomers and a second initiator.
[0061] Among them, in the second mixed monomer, the acrylic monomer includes acrylic acid and / or methacrylic acid; the acrylic ester monomer includes at least one of methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, cyclohexyl methacrylate and isobornyl methacrylate; the hydroxyl-containing acrylic ester monomer includes at least one of hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate and hydroxybutyl (meth)acrylate.
[0062] In a specific embodiment of the present invention, in the second mixed monomer, the mass proportion of the hydroxyl-containing acrylate monomer is 20% to 50%, such as 20%, 30%, 40%, 50% or a range consisting of any two thereof. In the second mixed monomer, the mass proportion of the acrylic monomer is 10% to 30%, such as 10%, 15%, 20%, 25%, 30% or a range consisting of any two thereof.
[0063] In a specific embodiment of the present invention, in the second mixed monomer, the second initiator includes a peroxide initiator, such as at least one of tert-butyl perbenzoate, di-tert-butyl hydroperoxide, and di-tert-amyl peroxide. The amount of the second initiator can be 0.1% to 3% of the mass of each monomer in the second mixed monomer, but is not limited thereto.
[0064] In a specific embodiment of the present invention, after the second mixed monomer is added and the reaction is carried out under heat preservation, a solution containing an initiator is further added. The type of initiator includes a peroxide initiator, and the solvent used in the solution includes at least one of ethylene glycol butyl ether and propylene glycol butyl ether. The amount of the added initiator can be 5wt% to 40wt% of the total mass of the first initiator and the second initiator, but is not limited thereto.
[0065] In a specific embodiment of the present invention, in step (a), the ratio of the sum of the mass of the first mixed monomer and the second mixed monomer to the mass of the PMMA microspheres is 1:(0.2-1).
[0066] For example, in different embodiments, in step (a), the ratio of the mass of the first mixed monomer and the second mixed monomer to the mass of the PMMA microspheres can be 1:0.2, 1:0.3, 1:0.4, 1:0.5, 1:0.6, 1:0.7, 1:0.8, 1:0.9, 1:1 or a range consisting of any two of them.
[0067] In a specific embodiment of the present invention, the mass ratio of the first mixed monomer to the second mixed monomer is (1.5-3):1.
[0068] For example, in different embodiments, the mass ratio of the first mixed monomer to the second mixed monomer may be 1.5:1, 1.8:1, 2:1, 2.2:1, 2.5:1, 2.8:1, 3:1 or a range consisting of any two of them.
[0069] In a specific embodiment of the present invention, in step (a), the temperature of the heat preservation reaction can be 120 to 145° C. The heat preservation reaction time can be 0.5 to 2 hours.
[0070] In a specific embodiment of the present invention, the neutralizing agent includes at least one of triethylamine, triethanolamine and N,N-dimethylethanolamine.
[0071] The amount of the neutralizer used may be 1 to 1.5 times the mass of the acrylic ester monomer in the second mixed monomer.
[0072] In a specific embodiment of the present invention, in step (b), the amount of water is adjusted so that the solid content of the self-matting acrylic dispersion is 40% to 50%, such as 45% to 48%. In actual operation, when adding water for dispersion, the first 1 / 3 of the water can be added slowly.
[0073] Another aspect of the present invention provides a self-matting acrylic dispersion prepared by any one of the above-mentioned methods for preparing a self-matting acrylic dispersion.
[0074] In a specific embodiment of the present invention, the solid content of the self-matting acrylic dispersion is ≥45%, such as 45% to 48%.
[0075] The self-matting acrylic dispersion of the present invention has a high solid content and excellent fullness.
[0076] Another aspect of the present invention provides a coating comprising any one of the above self-matting acrylic dispersions.
[0077] In a specific embodiment of the present invention, the coating further comprises an isocyanate curing agent.
[0078] In a specific embodiment of the present invention, in the coating, the equivalent ratio of the dispersion in terms of hydroxyl group to the isocyanate group in the isocyanate curing agent is 1:(1-2).
[0079] In actual operation, the coating may include component A and component B, wherein component A includes a self-matting acrylic dispersion, an optional color paste and an optional auxiliary agent, and component B includes an isocyanate curing agent. The color paste and the auxiliary agent may adopt conventional compositions of existing coatings.
[0080] The coating application method includes: mixing component A and component B, spraying under certain temperature and humidity conditions, leveling at room temperature for 10 to 30 minutes, and then baking at 70 to 75°C for 3.5 to 4 hours.
[0081] Example 1
[0082] This embodiment provides a method for preparing a self-matting acrylic dispersion, comprising the following steps:
[0083] (1) The solvent is added to a reaction kettle equipped with a stirrer, a thermometer, a serpentine condenser, and a constant pressure dropping funnel, and then the temperature is raised to 110°C, and component A is added dropwise to the reaction kettle. The addition is completed over 3 hours, and then the temperature is kept at 110°C for 1 hour to obtain a suspension containing PMMA microspheres. The corresponding glass transition temperature of the PMMA microspheres is 105°C, and D10, D50, and D90 are 5 μm, 10 μm, and 20 μm, respectively.
[0084] (2) The suspension containing PMMA microspheres obtained in step (1) is heated to 140° C., component B is added dropwise at a uniform rate within 3 hours, and then the mixture is kept at 140° C. for 20 minutes; component C is added dropwise to the reaction kettle at 140° C. within 2 hours, and the mixture is kept at 140° C. for 1 hour after the addition is completed; component D is added dropwise to the reaction kettle at a uniform rate within 2 minutes, and the mixture is kept at 140° C. for 1.5 hours after the addition is completed; the temperature is lowered to 120° C., component E is added dropwise to the reaction kettle within 2 minutes, and the mixture is stirred for 2 minutes, and then component F is added within 15 minutes for dispersion, and the mixture is stirred at about 55° C. for 1 hour to obtain a self-matting acrylic secondary dispersion having a solid content of 46% and a hydroxyl content of 3.3%.
[0085] The composition and dosage of each component in steps (1) and (2) are shown in Table 1.
[0086] Table 1 Composition and dosage of each component
[0087]
[0088] Example 2
[0089] This embodiment provides a method for preparing a self-matting acrylic dispersion, comprising the following steps:
[0090] (1) The solvent was added to a reaction kettle equipped with a stirrer, a thermometer, a serpentine condenser, and a constant pressure dropping funnel, and then the temperature was raised to 115°C, and component A was added dropwise to the reaction kettle. The addition was completed over 3 hours, and then the temperature was kept at 115°C for 1.5 hours to obtain a suspension containing PMMA microspheres. The corresponding glass transition temperature of the PMMA microspheres was 110°C, and D10, D50, and D90 were 5.5 μm, 10.3 μm, and 19.8 μm, respectively.
[0091] (2) The suspension containing PMMA microspheres obtained in step (1) is heated to 140° C., component B is added dropwise at a uniform rate within 4 hours, and then the mixture is kept at 140° C. for 30 minutes; component C is added dropwise to the reaction kettle at 140° C. within 2 hours, and the mixture is kept at 140° C. for 30 minutes after the addition is completed; component D is added dropwise to the reaction kettle at a uniform rate within 2 minutes, and the mixture is kept at 140° C. for 1.5 hours after the addition is completed; the temperature is lowered to 120° C., component E is added to the reaction kettle, and the mixture is stirred for 2 minutes, and then component F is added within 15 minutes for dispersion, and the mixture is stirred at about 55° C. for 1 hour to obtain a self-matting acrylic secondary dispersion having a solid content of 45% and a hydroxyl content of 2.2%.
[0092] The composition and dosage of each component in steps (1) and (2) are shown in Table 2.
[0093] Table 2 Composition and dosage of each component
[0094]
[0095]
[0096] Example 3
[0097] This embodiment provides a method for preparing a self-matting acrylic dispersion, comprising the following steps:
[0098] (1) The solvent is added to a reaction kettle equipped with a stirrer, a thermometer, a serpentine condenser, and a constant pressure dropping funnel, and then the temperature is raised to 115°C, and component A is added dropwise to the reaction kettle. The addition is completed over 3 hours, and then the temperature is kept at 115°C for 1.5 hours to obtain a suspension containing PMMA microspheres. The corresponding glass transition temperature of the PMMA microspheres is 110°C, and D10, D50, and D90 are 4.8 μm, 9.5 μm, and 21 μm, respectively.
[0099] (2) The suspension containing PMMA microspheres obtained in step (1) is heated to 140° C., component B is added dropwise at a uniform rate within 4 hours, and then the mixture is kept at 140° C. for 30 minutes; component C is added dropwise to the reaction kettle at 140° C. within 2 hours, and the mixture is kept at 140° C. for 30 minutes after the addition is completed; component D is added dropwise to the reaction kettle at a uniform rate within 2 minutes, and the mixture is kept at 140° C. for 1.5 hours after the addition is completed; the temperature is lowered to 120° C., component E is added to the reaction kettle, and the mixture is stirred for 2 minutes, and then component F is added within 15 minutes for dispersion, and the mixture is stirred at about 55° C. for 1 hour to obtain a self-matting acrylic secondary dispersion having a solid content of 48% and a hydroxyl content of 2.0%.
[0100] The composition and dosage of each component in steps (1) and (2) are shown in Table 3.
[0101] Table 3 Composition and dosage of each component
[0102]
[0103]
[0104] Embodiments 4 to 6
[0105] This embodiment provides a varnish and a preparation method thereof. The varnish comprises component A and component B; component A comprises a self-matting acrylic dispersion and an auxiliary agent; and component B comprises polyisocyanate.
[0106] The composition of the varnish is shown in Table 4.
[0107] Table 4 Composition of varnish
[0108]
[0109]
[0110] The preparation method of the coating comprises the following steps: firstly, adding a self-matting acrylic dispersion into a container, then adding an auxiliary agent under stirring, stirring for 15 minutes after the addition, standing for defoaming for 10 minutes, and obtaining component A; then adding a curing agent into component A, stirring evenly to obtain a paint sample.
[0111] Comparative Example 1
[0112] Comparative Example 1 provides a method for preparing an acrylic dispersion, comprising the following steps:
[0113] The solvent is added into a reaction kettle equipped with a stirrer, a thermometer, a serpentine condenser and a constant pressure dropping funnel, and then the temperature is raised to 140°C, component A is uniformly added dropwise within 4 hours, and the mixture is kept warm for 30 minutes after the addition is completed, and component B is uniformly added dropwise within 2 hours, and the mixture is kept warm at 140°C for 30 minutes after the addition is completed; component C is uniformly added dropwise into the reaction kettle within 2 minutes, and the mixture is kept warm for 1.5 hours after the addition is completed; the temperature is lowered to 120°C, component D is added into the reaction kettle, and after stirring for 2 minutes, component E is added within 15 minutes for dispersion, and the mixture is stirred at about 55°C for 1 hour to obtain an acrylic secondary dispersion with a solid content of 45% and a hydroxyl content of 3.3%.
[0114] The composition and dosage of each component are shown in Table 5.
[0115] Table 5 Composition and dosage of each component
[0116]
[0117] Comparative Example 2
[0118] Comparative Example 2 provides a method for preparing an acrylic dispersion, referring to Example 1, except that the preparation of the suspension containing PMMA microspheres in step (1) is different.
[0119] The step (1) of comparative example 2 comprises: adding 25 g of ethylene glycol butyl ether (BCS) into a reaction kettle equipped with a stirrer, a thermometer, a serpentine condenser, and a constant pressure dropping funnel, then raising the temperature to 110° C., dripping component A into the reaction kettle, and completing the dripping for 3 hours, and then keeping the temperature at 110° C. for 1 hour to obtain a suspension containing PMMA microspheres. The corresponding glass transition temperature of the PMMA microspheres is 65° C., and D10, D50, and D90 are 15 μm, 22 μm, and 29 μm, respectively.
[0120] Component A is 60 g of methyl methacrylate (MMA), 15 g of butyl acrylate, 5 g of trimethylolpropane trimethacrylate and 0.45 g of BPO initiator.
[0121] Comparative Examples 3-4
[0122] Comparative Examples 3 to 4 refer to the preparation method of Example 4, except that the dispersion prepared in Example 1 used in Example 4 is replaced by the dispersions prepared in Comparative Examples 1 to 2 in equal weights.
[0123] Experimental Example 1
[0124] The varnishes of Examples 4 to 6 and Comparative Examples 3 to 4 were sprayed on the surface of the tinplate which had been previously polished with 400-mesh sandpaper and wiped clean with anhydrous ethanol. The specific construction conditions are shown in Table 6.
[0125] Table 6 Construction conditions
[0126] temperature 24℃ humidity 48% Coating method Air spray Baking process Leveling at room temperature for 20 minutes, baking at 70℃ for 4 hours
[0127] The obtained paint film was subjected to performance tests, and the test results are shown in Table 7.
[0128] Table 7 Paint film performance test results
[0129] performance Example 4 Example 5 Example 6 Comparative Example 3 Comparative Example 4 Gloss (60°) 1.8 1 0.8 95 60 hardness H H 2H H H Adhesion Level 0 Level 0 Level 0 Level 0 0 Impact resistance (kg·cm) 50 50 40 40 50 Aging resistance (h) 1000 1000 1500 1000 800 Water resistance (h) 480 500 600 720 400 <![CDATA[Resistant to 5% H 2 SO 4 (h)]]> >48 >48 >72 >72 >72 Paint film appearance Matte, delicate Matte, delicate Matte, delicate Highlight Semi-matte
[0130] The performance evaluation standards are as follows:
[0131] Gloss: GB / T 9754-2007;
[0132] Hardness: GB / T 6739-2006;
[0133] Adhesion: GB / T 9286-1998;
[0134] Impact resistance: GB1732-79 (88);
[0135] Aging resistance: GB / T 1766-2008, the maximum time that can be achieved without the gloss loss rate exceeding 20% and without discoloration;
[0136] Water resistance: GB / T 1733-2013, the maximum time that can be achieved without blistering or shedding (slight discoloration is allowed);
[0137] Resistant to 5% H 2 SO 4 : Place the test plate in 5% H 2 SO 4 After a certain period of time in an acidic solution, observe the changes in the coating, such as discoloration, peeling or blistering. Taking ">48" as an example, it means that the test plate is placed in 5% H 2 SO 4 After 48 hours in acidic solution, there will be no discoloration, peeling or bubbles.
[0138] From the above test results, it can be seen that the PMMA microspheres of the self-matting acrylic dispersion synthesized by the present invention can be well dispersed in the acrylic dispersion, and when preparing the paint film, they can be suspended on the surface of the paint film to achieve excellent matting effect, and can solve the problem of whitening and fogging of the paint film caused by conventional addition of matting aids, and improve the permeability of the paint film. At the same time, the self-matting acrylic dispersion synthesized by the present invention has good stability, and the appearance of the prepared paint film is excellent, and has excellent adhesion, hardness, impact resistance, aging resistance, water resistance and corrosion resistance.
[0139] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a self-matting acrylic dispersion, characterized in that: The steps include: (a) adding a first mixed monomer to a suspension containing PMMA microspheres and then incubating the mixture for reaction, and then adding a second mixed monomer and then incubating the mixture for reaction; (b) adding a neutralizing agent to the system obtained in step (a) to carry out a neutralization reaction, and then adding water to disperse the system to obtain the self-matting acrylic dispersion; The PMMA microsphere-containing suspension is mainly prepared from methyl methacrylate, a cross-linking monomer, a solvent, an initiator and an optional copolymer monomer; the glass transition temperature of the PMMA microsphere is ≥90° C., and the average particle size D50 of the PMMA microsphere is 5 to 15 μm.
2. The method for preparing the self-matting acrylic dispersion according to claim 1, characterized in that: In the preparation of the suspension containing PMMA microspheres, the mass ratio of the methyl methacrylate to the cross-linking monomer is 1:(0.1-0.5); Preferably, the crosslinking monomer includes at least one of trimethylolpropane trimethacrylate and 1,6-hexanediol diacrylate.
3. The method for preparing the self-matting acrylic dispersion according to claim 1, characterized in that: The comonomer comprises at least one of styrene, cyclohexyl methacrylate, butyl methacrylate, isobornyl methacrylate, butyl acrylate, isooctyl acrylate, hydroxyethyl methacrylate, hydroxyethyl acrylate, hydroxypropyl methacrylate, propyl acrylate and methacrylic acid; Preferably, the mass of the comonomer is 0% to 40% of the mass of the methyl methacrylate.
4. The method for preparing the self-matting acrylic dispersion according to claim 1, characterized in that: The particle size of the PMMA microspheres meets at least one of the following characteristics: (1) D10 is 3 to 7 μm; (2) D90 is 15 to 25 μm; Preferably, the particle size distribution of the PMMA microspheres is approximately normal distribution.
5. The method for preparing the self-matting acrylic dispersion according to claim 1, characterized in that: The first mixed monomer includes any one or more of an acrylate monomer, a hydroxyl-containing acrylate monomer and a vinyl monomer, and a first initiator; And / or, the second mixed monomer includes acrylic monomers, acrylate monomers, hydroxyl-containing acrylate monomers and a second initiator; Preferably, the first mixed monomer does not include a copolymerizable monomer containing a carboxyl group.
6. The method for preparing the self-matting acrylic dispersion according to claim 1, characterized in that: In step (a), the ratio of the sum of the mass of the first mixed monomer and the second mixed monomer to the mass of the PMMA microspheres is 1:(0.2-1).
7. The method for preparing the self-matting acrylic dispersion according to claim 1, characterized in that: The neutralizing agent includes at least one of triethylamine, triethanolamine and N,N-dimethylethanolamine.
8. A self-matting acrylic dispersion prepared by the method for preparing a self-matting acrylic dispersion according to any one of claims 1 to 7.
9. The self-matting acrylic dispersion according to claim 8, characterized in that The self-matting acrylic dispersion has a solid content of ≥45%.
10. A coating, characterized in that: The invention comprises the self-matting acrylic dispersion prepared by the preparation method according to any one of claims 1 to 7 or the self-matting acrylic dispersion according to any one of claims 8 to 9.