Solvent-resistant, recoverable and self-repairing polyurethane elastomer and preparation method thereof

By using ascorbic acid as a chain extender and ketone and enol structure in polyurethane materials, combined with solution polymerization method and prepolymer method, solvent-resistant, recyclable and self-repaired polyurethane elastomer was prepared, which solved the problem of existing materials at normal temperature. The problem of easy corrosion and difficulty in recycling has achieved high solvent resistance and recyclability of the material, reducing resource waste.

CN118994526AActive Publication Date: 2024-11-22BEIJING INST OF TECH

Patent Information

Application Number
CN202411243949.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-11-22
Estimated Expiration
2044-09-05

AI Technical Summary

Technical Problem

Existing self-repaired polyurethane materials are susceptible to corrosion by organic solvents at room temperature, resulting in swelling or dissolution, and are difficult to recycle and use, resulting in waste of resources, and violate the concept of sustainable development.

Method used

Using ascorbic acid as a chain extender, combining the dynamic transformation of ketone and enol structures, polyurethane elastomers are prepared through solution polymerization and prepolymer methods, improving the self-healing ability and structural stability of the material, and using DMF as solvent to reduce The viscosity of the reaction system and can be re-sampled at high temperatures for recovery.

Benefits of technology

The material exhibits high solvent resistance among a variety of organic solvents, does not swell at room temperature, can be dissolved and re-formed at high temperature, and can recover the mechanical properties, realizing the recyclable and degradable properties of the material and reducing resource waste.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994526A_ABST
    Figure CN118994526A_ABST
Patent Text Reader

Abstract

The invention relates to a solvent-resistant, recoverable and self-repairing polyurethane elastomer and a preparation method thereof, and belongs to the technical field of high-performance polymers. A novel cross-linking system is found by using ascorbic acid as a chain extender, and compared with a common chain extender BDO, ascorbic acid can provide enough chemical cross-linking points to form a polyurethane elastomer with better mechanical properties, so that the polyurethane elastomer only swells and is not dissolved in various organic solvents at normal temperature. Therefore, the material can be applied to various complex environments. Dynamic balance of ketone and enol structure transformation exists in ascorbic acid, so that the obtained polyurethane elastomer has a self-repairing function, fractures are spliced after a test sample strip is broken, preliminary healing can be realized in a short time, and the self-repairing efficiency is not lower than 29% after repairing is performed for one day at normal temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a solvent-resistant, recyclable, self-repairing polyurethane elastomer and a preparation method thereof, belonging to the technical field of high-performance polymers. Background Art

[0002] Polyurethane elastomers are widely used in various fields such as national defense, military industry and civil construction due to their excellent performance. It is a macromolecular polymer formed by the chemical reaction between the hydroxyl group (-OH) of the polyol and the isocyanate group (-NCO) of the polyisocyanate to form a carbamate (-NH-COO-) group in the molecular chain. It is a typical block polymer composed of alternating soft segments and hard segments. The interaction between the soft and hard segments makes it show microphase separation and supramolecular network. Among them, the soft segment is composed of long molecular chain flexible polyether polyols, accounting for 50% to 90%, and the hard segment is composed of isocyanates and small molecule chain extenders, accounting for about 10% to 50%. A large number of hydrogen bonds can be formed between the carbamate groups in the hard segment corresponding to the isocyanate and the chain extender. These hydrogen bonds play a physical cross-linking effect to form hard segment micro-regions. The soft segment and the hard segment are thermodynamically incompatible, which leads to a microphase separation structure in the aggregated state. These unique structures give polyurethane elastomers excellent properties. The soft segment gives polyurethane good elasticity and low temperature resistance, while the hydrogen bonds in the hard segment can make it wear-resistant, tough and have a small tensile permanent deformation. Polyurethane elastomers have excellent comprehensive properties. Compared with metal materials, they are low in weight, corrosion-resistant, simple to process, and have good sound insulation and shock absorption. Compared with general rubber, they have the advantages of cutting resistance, ozone resistance, tear resistance, transparency, various preparation methods, and a wide range of hardness.

[0003] However, during the use of materials, due to the influence of mechanical, chemical, thermal and other factors, microcracks or macro fractures will inevitably occur, which will affect the service life of the materials and even pose safety hazards. The self-healing ability of polymers has become a research hotspot in recent years. Self-healing materials refer to materials that can repair damaged parts without intervention or under certain stimulation (light, heat, electricity, microwave, etc.) after being damaged, thereby restoring their original state. The significance of self-healing for polymer materials is to improve the durability, reliability and safety of materials while reducing maintenance costs. In principle, the self-healing types of materials are generally divided into external aid type and intrinsic type. The former relies on microcapsules or liquid core fibers containing repair agents pre-buried in the matrix to achieve repair, while the latter has repeatable self-healing ability, which only relies on the physical and chemical properties of the material itself (such as molecular diffusion, reversible covalent bonds, reversible non-covalent bonds) to repair the material. Compared with external aid self-healing, intrinsic self-healing materials are simple to prepare, and because the internal dynamic bonds can be dynamically reorganized, they can simultaneously give the material recyclable and degradable properties.

[0004] However, the currently common self-healing polyurethane has many shortcomings: it is easily corroded by organic solvents at room temperature, causing substantial swelling or even dissolution, and it is difficult to recycle after use, resulting in a lot of waste of resources, which is not in line with the current concept of sustainable development. Summary of the invention

[0005] In view of the defects existing in the technical field at present, the present invention provides a solvent-resistant, recyclable, self-repairing polyurethane elastomer and a preparation method thereof. The polyurethane elastomer uses ascorbic acid as a chain extender, and there is a dynamic transformation between ketone and enol structures inside. The four hydroxyl groups of ascorbic acid provide enough chemical crosslinking points, and this unique chemical structure gives the polyurethane material the ability to self-repair. At the same time, the crosslinking structure improves the structural stability of the polyurethane, and has better solvent resistance than general polyurethane materials. The swelling rate in a variety of organic solvents at room temperature is extremely small or even non-swelling. It is soluble in general organic solvents at high temperatures, and can be re-sampled after evaporating the solvent. The mechanical properties of the sample can be restored after recycling, and it has a very high elongation at break. The recyclable performance enables the material to effectively reduce resource waste. With polytetramethylene glycol (PTMG) as the soft segment, isophorone diisocyanate (IPDI) and ascorbic acid as the hard segment, the solution polymerization method is used for polymerization, and DMF is used as the solvent in the reaction process to reduce the viscosity of the reaction system. The prepolymer method is used for polymerization, and PTMG needs to be dehydrated before use. First, add the measured PTMG and IPDI to a three-necked flask, drop a trace amount of DBTDL as a catalyst to accelerate the polymerization reaction, and obtain an isocyanate-terminated polyurethane prepolymer after the reaction is completed; after the temperature drops, add DMF as the reaction solvent, add the measured ascorbic acid powder, and continue the reaction to obtain the final product. The product is cast into a preheated polytetrafluoroethylene mold and used for subsequent testing after curing.

[0006] To achieve the above objectives, the technical solution of the present invention is as follows.

[0007] A solvent-resistant, recyclable, self-repairing polyurethane elastomer, the raw materials of which include ascorbic acid chain extender, polytetramethylene glycol (PTMG), isophorone diisocyanate (IPDI), N,N-dimethylformamide (DMF) solvent, and dibutyltin dilaurate (DBTDL);

[0008] Taking the sum of the mass of ascorbic acid chain extender, polytetramethylene glycol (PTMG), isophorone diisocyanate (IPDI) and dibutyltin dilaurate (DBTDL) as 100%, the percentage content of each component is:

[0009] Ascorbic acid chain extender 3%-4%;

[0010] Polytetramethylene glycol (PTMG) 75%-80%;

[0011] Isophorone diisocyanate (IPDI) 15%-20%;

[0012] Dibutyltin dilaurate (DBTDL) 0.1%-0.3%;

[0013] The ratio of N,N-dimethylformamide (DMF) solvent to polytetrahydrofuran diol is 10-30mL:15g;

[0014] The molecular weight of described polytetrahydrofuran diol is 2000g / mol.

[0015] A method for preparing a solvent-resistant, recyclable, self-repairing polyurethane elastomer, the method comprising the steps of:

[0016] The first step is to dehydrate polytetrahydrofuran diol (PTMG);

[0017] The second step is to mix and stir the polytetrahydrofuran diol (PTMG), isophorone diisocyanate (IPDI) and dibutyltin dilaurate (DBTDL) after the dehydration treatment in the first step to react at a mixing temperature of 80-90° C., a stirring speed of 220-300 r / min, and a stirring time of 2-4 h, and after the reaction is completed, a prepolymer of an isocyanate-terminated polyurethane is obtained;

[0018] The third step is to mix the ascorbic acid chain extender and the N,N-dimethylformamide (DMF) solvent to obtain a mixture;

[0019] The fourth step is to mix and stir the mixture obtained in the third step with the prepolymer obtained in the second step to react, the mixing temperature is 80-90°C, the stirring speed is 220-300r / min, and the stirring time is 4-6h. After the reaction is completed, the product is dried at a drying temperature of 75-85°C and a drying time of 1-2 days to obtain a solvent-resistant, recyclable, self-healing polyurethane elastomer.

[0020] After the solvent-resistant, recyclable, self-repairing polyurethane elastomer is used, if it is damaged, the method for recycling is as follows:

[0021] The used solvent-resistant, recyclable, self-healing polyurethane elastomer is cut into pieces and mixed with N,N-dimethylformamide (DMF) solvent to obtain mixture A, which is sealed with plastic wrap and placed in an oven with a temperature set at 80-100°C. After the sample is completely dissolved, several small holes are pierced in the plastic wrap to evaporate part of the solvent to obtain mixture B, the mass of which is 10%-15% of the mass of mixture A. Mixture B is then dried at a drying temperature of 75-85°C for 1-2 days to obtain the solvent-resistant, recyclable, self-healing polyurethane elastomer.

[0022] Beneficial Effects

[0023] The present invention provides a method for preparing a solvent-resistant, recyclable, self-repairing polyurethane elastomer. The terminal group of the diisocyanate in the raw material is an isocyanate group, and the terminal group of the polyether polyol is a hydroxyl group. After the mixed reaction, an isocyanate-terminated polyurethane prepolymer is obtained, and the prepolymer can subsequently react with a variety of small molecule chain extenders such as alcohols and amines, and can be flexibly adjusted according to the experimental formula design. The method is simple to operate and can be used for laboratory preparation and industrial production.

[0024] The present invention provides a method for preparing a solvent-resistant, recyclable, self-repairing polyurethane elastomer. Using ascorbic acid as a chain extender, a new cross-linking system is discovered. Compared with the common chain extender BDO, ascorbic acid can provide enough chemical cross-linking points to form a polyurethane elastomer with better mechanical properties, so that it only swells but does not dissolve in a variety of organic solvents at room temperature. This allows the material to be applied in a variety of complex environments.

[0025] The present invention provides a method for preparing a solvent-resistant, recyclable, self-repairing polyurethane elastomer. Due to the dynamic balance of ketone and enol structural transformation inside ascorbic acid, the obtained polyurethane elastomer has a self-repairing function. After the test specimen is broken, the fracture is spliced ​​and preliminary healing can be achieved in a short time. The self-repairing efficiency is not less than 29% after one day of repair at room temperature.

[0026] The present invention provides a method for recycling a solvent-resistant, recyclable, and self-repairing polyurethane elastomer. After the original sample is dissolved at high temperature, it is recast into a sample, and the polyurethane elastomer can still be formed, and its mechanical properties can be restored to a certain extent, while showing super-stretching properties, which can effectively reduce resource waste and is conducive to sustainable development. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 is the infrared spectrum of the polyurethane obtained in the comparative example;

[0028] Figure 2 Infrared spectrum of solvent-resistant, recyclable, self-healing polyurethane elastomer;

[0029] Figure 3 This is a self-healing result diagram of a solvent-resistant, recyclable, self-healing polyurethane elastomer;

[0030] Figure 4 This is a comparison chart of the mechanical properties of the solvent-resistant, recyclable, self-healing polyurethane elastomer before and after self-healing;

[0031] Figure 5 Cyclic stretching diagram for solvent-resistant, recyclable, self-healing polyurethane elastomer;

[0032] Figure 6 This is a test diagram of the swelling rate of solvent-resistant, recyclable, and self-healing polyurethane elastomer in three organic solvents;

[0033] Figure 7 This is a test diagram of the mechanical properties of the reshaped solvent-resistant, recyclable, and self-healing polyurethane elastomer. DETAILED DESCRIPTION

[0034] The present invention is described in detail below in conjunction with the accompanying drawings, which is not intended to limit the patent of the present invention.

[0035] Example

[0036] A method for preparing a solvent-resistant, recyclable, self-repairing polyurethane elastomer, comprising:

[0037] 1. Raw material dehydration: Water in polytetrahydrofuran diol (PTMG) will react with isocyanate. In order to eliminate the interference of water, it is dehydrated. Weigh 100g PTMG into a 250ml three-necked flask, add a magnetic rotor, set the oil bath temperature to 105℃, the speed to 250r / min, connect a vacuum pump to dehydrate for 2 hours, and pour it into a tetrafluoroethylene bottle for standby use after dehydration.

[0038] 2. Preparation of prepolymer: Weigh 7.5mmol (15.00g) PTMG and 15mmol (3.3348g) IPDI, add them into a 250ml three-necked flask, drop 0.04g DBTDL as a catalyst, set the temperature to 85℃, rotate at 250r / min, and react for 4 hours to obtain an isocyanate-terminated polyurethane prepolymer.

[0039] 3. Chain extension: Weigh 3.75 mmol (0.66 g) of ascorbic acid powder into a glass beaker, add 20 g of DMF, and add the solution to the above prepolymer after the ascorbic acid is dissolved. Set the polymerization temperature to 85°C, the speed to 250 r / min, and react for 4 hours. Pour the reaction product into a tetrafluoroethylene evaporating dish, set the temperature to 80°C, evaporate the residual solvent in an oven, and cure for two days.

[0040] The obtained product is a brown-red polyurethane elastomer, and its infrared spectrum test results are as follows: Figure 2 As shown. 2271cm -1 There is no characteristic absorption peak at 3325cm -1 and 1110cm -1 The peaks that appeared correspond to the stretching vibration peaks of NH and COC of the carbamate group. The disappearance and appearance of the above peaks indicate that the polyurethane was successfully prepared.

[0041] The specimen was cut short in the middle and then spliced ​​along the fracture, and preliminary healing was achieved. Figure 3 The cut dumbbell specimens are used for mechanical tensile testing, as shown in Figure 4 As shown, when the loading rate is set to 200 mm / min, the elongation at break can reach 1432.832%, and the fracture strength is 11.537 MPa. The broken specimens are quickly spliced ​​along the fracture. After repairing at room temperature for 1 day, they are tested again under the same conditions. The fracture strength is 3.361 MPa and the self-repair efficiency is 29.1%.

[0042] The results of cyclic stretching are as follows Figure 5 As shown in the figure, the loading rate is set at 200 mm / min, and the deformation of each cycle gradually increases from 100% to 400%. The sample shows a hysteresis loop, and the hysteresis energy gradually increases as the strain increases to 400%. After loading several times, the spline can recover its original length in a short time, showing good resilience.

[0043] The samples were cut with a square cutter for swelling test to investigate the solubility of polyurethane elastomer in three organic solvents, namely N, N-dimethylformamide (DMF), N, N-dimethylacetamide (DMAC), and dimethyl sulfoxide (DMSO). In the experiment, the sample was first weighed when dry, immersed in the solvent, and after the swelling equilibrium was reached and the solvent evaporated completely, its weight was recorded again. The results showed that at room temperature, the prepared polyurethane elastomer only swelled but did not dissolve in these three organic solvents, and had good solvent resistance. The test results are shown in Table 1 and Figure 6 As shown: the obtained polyurethane elastomer swells most significantly in N,N-dimethylformamide, with a swelling rate of 213.6%; N,N-dimethylacetamide is second, with a swelling rate of 143.9%; and the swelling degree is the smallest in dimethyl sulfoxide, with a swelling rate of 54.1%.

[0044] Table 1 Swelling test results of polyurethane in organic solvents

[0045] Solvent type Starting mass (mg) Balance mass (mg) Swelling rate (%) N,N-Dimethylformamide 175.8 551.4 213.6 N,N-Dimethylacetamide 176.3 430.9 143.9 Dimethyl sulfoxide 173.6 264.2 52.1

[0046] The recovery method of the obtained polyurethane is:

[0047] Cut all the waste samples after the test into pieces, pour them into a 500ml beaker, add 250g DMF, seal with plastic wrap, put into an oven, set the temperature to 100℃, and after the sample is completely dissolved, poke several small holes in the plastic wrap, evaporate part of the solvent until the solution reaches 75g, then pour the solution into a tetrafluoroethylene mold and put it into an oven to evaporate the residual solvent, set the temperature to 80℃, and cure for two days to obtain the reshaped sample.

[0048] Use a cutter to cut dumbbell specimens for mechanical tensile testing at a loading rate of 200 mm / min. The test results are as follows: Figure 7 The breaking strength is 7.594MPa, the breaking elongation is 2588%, and the overall recycling efficiency is 65.8%.

[0049] Comparative Example

[0050] The common chain extender 1,4-butanediol (BDO) was used for chain extension.

[0051] 1. Raw material dehydration: Water in polytetrahydrofuran diol (PTMG) will react with isocyanate. In order to eliminate the interference of water, it is dehydrated. Weigh 100g PTMG into a 250ml three-necked flask, add a magnetic rotor, set the oil bath temperature to 105℃, the speed to 250r / min, connect a vacuum pump to dehydrate for 2 hours, and pour it into a tetrafluoroethylene bottle for standby use after dehydration.

[0052] 2. Preparation of prepolymer: Weigh 7.5mmol (15.00g) PTMG and 15mmol (3.3348g) IPDI, add them into a 250ml three-necked flask, drop 0.04g DBTDL as a catalyst, set the temperature to 85℃, rotate at 250r / min, and react for 4 hours to obtain an isocyanate-terminated polyurethane prepolymer.

[0053] 3. Chain extension: Weigh 7.5 mmol (0.675 g) of BDO into a glass beaker, add 20 g of DMF, and add the solution to the above prepolymer after BDO is dissolved. Set the polymerization temperature to 85°C, the speed to 250 r / min, and react for 4 hours. Pour the reaction product into a tetrafluoroethylene evaporating dish, set the temperature to 80°C, evaporate the residual solvent in an oven, and cure for two days.

[0054] The obtained product was slightly yellow and sticky, and was difficult to use for mechanical testing. A small amount of sample was taken for infrared spectroscopy testing, and the results were as follows: Figure 1 shown.

[0055] In summary, the above are only preferred embodiments of the present invention and are not intended to limit the protection scope of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A solvent-resistant, recyclable, self-healing polyurethane elastomer, characterized in that: The raw materials of the polyurethane elastomer include ascorbic acid chain extender, polytetramethylene glycol, isophorone diisocyanate, N,N-dimethylformamide and dibutyltin dilaurate; Taking the sum of the mass of ascorbic acid chain extender, polytetramethylene glycol, isophorone diisocyanate and dibutyltin dilaurate as 100%, the percentage content of each component is: Ascorbic acid chain extender 3%-4%; Polytetramethylene glycol 75%-80%; Isophorone diisocyanate 15%-20%; Dibutyltin dilaurate 0.1%-0.3%; The ratio of N,N-dimethylformamide to polytetrahydrofuran diol is 10-30mL:15g.

2. A solvent-resistant, recyclable, self-healing polyurethane elastomer according to claim 1, characterized in that: The molecular weight of described polytetrahydrofuran diol is 2000g / mol.

3. A method for preparing a solvent-resistant, recyclable, self-repairing polyurethane elastomer, characterized in that The steps of the method include: The first step is to dehydrate polytetrahydrofuran diol; The second step is to mix and stir the polytetrahydrofuran diol, isophorone diisocyanate and dibutyltin dilaurate after the dehydration treatment in the first step to react, and obtain an isocyanate-terminated polyurethane prepolymer after the reaction is completed; The third step is to mix the ascorbic acid chain extender and N,N-dimethylformamide to obtain a mixture; In the fourth step, the mixture obtained in the third step is mixed with the prepolymer obtained in the second step, stirred and reacted, and after the reaction is completed, the product is dried to obtain a solvent-resistant, recyclable, self-repairing polyurethane elastomer.

4. The method for preparing a solvent-resistant, recyclable, self-repairing polyurethane elastomer according to claim 3, characterized in that: In the second step, the mixing temperature is 80-90° C., the stirring speed is 220-300 r / min, and the stirring time is 2-4 h.

5. The method for preparing a solvent-resistant, recyclable, self-repairing polyurethane elastomer according to claim 3, characterized in that: In the fourth step, the mixing temperature is 80-90° C., the stirring speed is 220-300 r / min, and the stirring time is 4-6 h.

6. The method for preparing a solvent-resistant, recyclable, self-repairing polyurethane elastomer according to claim 3, characterized in that: In the fourth step, the drying temperature is 75-85° C. and the drying time is 1-2 days.

7. A method for recycling a solvent-resistant, recyclable, self-repairing polyurethane elastomer, characterized in that: The used solvent-resistant, recyclable, self-healing polyurethane elastomer is cut into pieces and mixed with N,N-dimethylformamide to obtain mixture A, which is sealed with plastic wrap and placed in an oven. After the sample is completely dissolved, several small holes are pierced in the plastic wrap to evaporate part of the solvent to obtain mixture B. The mass of mixture B is 10%-15% of the mass of mixture A. Mixture B is then dried to obtain the solvent-resistant, recyclable, self-healing polyurethane elastomer again.

8. The method for recycling a solvent-resistant, recyclable, self-repairing polyurethane elastomer according to claim 7, characterized in that: The ratio of the shredded self-healing polyurethane elastomer to N,N-dimethylformamide when mixed is 25g:200-250mL.

9. The method for recycling a solvent-resistant, recyclable, self-repairing polyurethane elastomer according to claim 7, characterized in that: The oven temperature is set to 80-100°C.

10. The method for recycling a solvent-resistant, recyclable, self-repairing polyurethane elastomer according to claim 7, characterized in that: The drying temperature is 75-85°C and the drying time is 1-2 days.

Citation Information

Patent Citations

  • Nerve film and preparation method thereof

    CN109867810A

  • Intravascular stent and preparation method thereof

    CN111467582A

  • Aqueous dispersions of polyurethane-addition polymer hybrid particles especially for use in coating compositions

    CN1729222A

  • Method for preparimg wear resistant polyurethane elastomer

    KR100943195B1

Cited By

  • Four-arm cross-linked polyurethane elastomer and preparation method thereof

    CN120923730A