MCA supramolecular aggregate hollow sphere as well as preparation method and application thereof

MCA supramolecular aggregate hollow spheres were prepared by combining melamine, cyanuric acid and soft template agent, and carbon nitride hollow spheres with controllable size were prepared, solving the complexity and environment of traditional template preparation methods. The risk issue has achieved simple, safe and controllable carbon nitride hollow sphere synthesis, expanding the application prospects of supramolecular pre-assembly method.

CN118994570APending Publication Date: 2024-11-22JIANGSU UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411092322.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The hard template preparation process of traditional carbon nitride hollow spheres is complicated, and the process of removing templates is prone to collapse of hollow structures. The use of strong hydrofluoroic acid poses environmental risks, making it difficult to achieve a simple process, safe and controllable, and complete hollow structure preparation method.

Method used

The mixture of melamine, cyanuric acid and soft template agent was used for constant temperature stirring and post-treatment to prepare MCA supramolecular aggregate hollow spheres. They were used as precursors to prepare controllable size and complete hollow structures by supramolecular pre-assembly method. carbon nitride hollow spheres.

Benefits of technology

The preparation of MCA supramolecular aggregate hollow spheres with simple process, easy raw materials, and no secondary pollution. The particle size is controllable and suitable for promotion and application. It has successfully prepared a complete structure of carbon nitride hollow sphere photocatalyst, expanding the super Application prospects of molecular preassembly method in the synthesis of hollow carbon nitride spheres.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994570A_ABST
    Figure CN118994570A_ABST
Patent Text Reader

Abstract

The invention provides an MCA supramolecular aggregate hollow sphere and a preparation method and application thereof, and belongs to the technical field of MCA preparation. Melamine, cyanuric acid and a solvent are mixed to obtain a mixed solution, then the mixed solution and a soft template agent are mixed, the shape and size are controlled through the soft template agent, constant-temperature stirring and aftertreatment are sequentially conducted, and the MCA supramolecular aggregate hollow sphere is obtained. And preparing the MCA supramolecular aggregate hollow sphere with controllable size. The method provided by the invention is simple in process, easily available and cheap in raw materials, easy to control, free of secondary pollution and suitable for popularization and application, the prepared MCA has a hollow spherical microstructure and a controllable particle size, and the MCA supramolecular aggregate hollow sphere is used as a precursor to prepare a carbon nitride hollow sphere with a controllable size and a complete hollow structure. The carbon nitride hollow sphere photocatalyst with a controllable size can be effectively prepared by a supramolecular preassembly method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of MCA preparation, and in particular to an MCA supramolecular aggregate hollow sphere and a preparation method and application thereof. Background Art

[0002] As a semiconductor photocatalyst, graphite carbon nitride (g-C3N4) has the advantages of high stability, safety and visible light response. The photocatalytic performance of carbon nitride hollow spheres is greatly improved due to their structural advantages of low density and large specific surface area. The traditional hard template preparation method of carbon nitride hollow spheres is complicated, and the template removal process is prone to cause the hollow structure to collapse. At the same time, a large amount of hydrofluoric acid etching is used, which poses certain environmental risks. Therefore, providing a preparation method for carbon nitride hollow spheres with a simple process, safe and controllable, and complete hollow structure is of great significance to improve the practical application of carbon nitride photocatalysts. Summary of the invention

[0003] The purpose of the present invention is to provide an MCA supramolecular aggregate hollow sphere and a preparation method and application thereof. The method provided by the present invention has simple process, readily available and inexpensive raw materials, easy control, and no secondary pollution. The prepared MCA has a hollow spherical microscopic morphology, good dispersibility, and controllable particle size. The MCA supramolecular aggregate hollow sphere can be used as a precursor to prepare carbon nitride hollow spheres with controllable size and complete hollow structure.

[0004] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0005] The present invention provides a method for preparing MCA supramolecular aggregate hollow spheres, comprising the following steps:

[0006] (1) mixing melamine, cyanuric acid and a solvent to obtain a mixed solution;

[0007] (2) The mixed solution in step (2) and the soft template are mixed, and the mixture is stirred at a constant temperature and post-treated in sequence to obtain hollow spheres of MCA supramolecular aggregates.

[0008] Preferably, the solvent in step (1) is one or more of ethylene glycol, dimethyl sulfoxide, glycerol, and N,N-dimethylformamide.

[0009] Preferably, in step (1), the concentrations of melamine and cyanuric acid in the mixed solution are equal; and the concentration of melamine in the mixed solution is 15 to 70 mmol·L.

[0010] Preferably, the soft template in step (2) is triblock copolymer P123.

[0011] Preferably, the temperature of the constant temperature stirring in step (2) is 25 to 130° C., and the time of the constant temperature stirring is 20 to 50 min.

[0012] Preferably, the post-treatment in step (2) comprises: centrifugation, washing and drying in sequence.

[0013] The invention provides a MCA supramolecular aggregate hollow sphere, which is obtained by the preparation method described in the above technical scheme; the MCA supramolecular aggregate hollow sphere is self-compounded by melamine and cyanuric acid through hydrogen bonds.

[0014] Preferably, the MCA supramolecular aggregate hollow sphere has a spherical microscopic morphology with a hollow structure, and the particle size thereof is 0.7 to 8 μm.

[0015] The present invention also provides the use of the MCA supramolecular aggregate hollow spheres described in the above technical solution in the preparation of carbon nitride hollow sphere photocatalysts.

[0016] The present invention provides a method for preparing hollow spheres of MCA supramolecular aggregates. After melamine, cyanuric acid and a solvent are mixed to obtain a mixed solution, the mixed solution and a soft template are mixed, and constant temperature stirring and post-treatment are performed in sequence to obtain hollow spheres of MCA supramolecular aggregates. The soft template method provided by the present application uses melamine and cyanuric acid as reactants, controls the morphology and size through a soft template, and prepares hollow spheres of MCA supramolecular aggregates with good dispersibility and controllable size. The method provided by the present invention has simple process, readily available and inexpensive raw materials, is easy to control, has no secondary pollution, is suitable for promotion and application, and the prepared MCA has a hollow spherical microscopic morphology and controllable particle size, which solves the dependence of the traditional template preparation method on the hard template, and uses the hollow spheres of MCA supramolecular aggregates as precursors to prepare hollow carbon nitride spheres with controllable size and complete hollow structure, so as to expand the realization of the supramolecular preassembly method to effectively prepare hollow carbon nitride sphere photocatalysts with controllable size. The results of the examples show that, using the method provided by the present invention, Example 1 successfully self-assembles and prepares MCA supramolecular aggregates with an average particle size of 1 μm having a hollow sphere structure, and, under the same constant temperature stirring temperature conditions, the particle size of the MCA supramolecular aggregate hollow spheres prepared in Examples 1 to 6 decreases with the increase of the concentration of the reactants (melamine and cyanuric acid), and under the same reactant concentration conditions, the particle size of the product increases with the increase of the constant temperature stirring temperature. By adjusting the type of solvent, the concentration of the raw materials melamine and cyanuric acid, and the constant temperature stirring temperature, the size of the product MCA supramolecular aggregate hollow spheres can be effectively controlled; Example 7 uses the MCA supramolecular aggregate hollow spheres prepared in Example 1 as a precursor, and successfully prepares carbon nitride hollow spheres with complete structure and high sphericity by using the supramolecular preassembly method. The method provided by the present invention has good application prospects in realizing controllable synthesis of carbon nitride hollow spheres by supramolecular preassembly. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 The X-ray diffraction pattern of the MCA supramolecular aggregate hollow sphere prepared in Example 1 of the present invention, wherein the abscissa represents the 2θ angle and the ordinate represents the intensity;

[0018] Figure 2 The Fourier transform infrared spectrum of the MCA supramolecular aggregate hollow sphere prepared in Example 1 of the present invention, wherein the abscissa represents the wave number and the ordinate represents the transmittance;

[0019] Figure 3 TEM image of the MCA supramolecular aggregate hollow sphere prepared in Example 1 of the present invention;

[0020] Figure 4 The SEM images of the hollow spheres of MCA supramolecular aggregates prepared in Examples 1 to 6 of the present invention are shown in FIG. Figure 4 (a) is MCA-20-30 in Example 1, Figure 4 (b) is MCA-40-30 in Example 2, Figure 4 (c) is MCA-60-30 in Example 3, Figure 4 (d) is MCA-40-60 in Example 4, Figure 4 (e) is MCA-40-100 in Example 5, Figure 4 (f) is MCA-40-120 in Example 6;

[0021] Figure 5 This is a SEM image of the hollow carbon nitride spheres prepared in Example 7 of the present invention. DETAILED DESCRIPTION

[0022] In the present invention, unless otherwise specified, the raw materials used are conventional commercial products in the art.

[0023] The present invention provides a method for preparing MCA supramolecular aggregate hollow spheres, comprising the following steps:

[0024] (1) mixing melamine, cyanuric acid and a solvent to obtain a mixed solution;

[0025] (2) The mixed solution in step (2) and the soft template are mixed, and the mixture is stirred at a constant temperature and post-treated in sequence to obtain hollow spheres of MCA supramolecular aggregates.

[0026] The invention mixes melamine, cyanuric acid and a solvent to obtain a mixed liquid.

[0027] In the present invention, the mixing temperature of melamine, cyanuric acid and solvent is preferably 25-130° C.; the mixing method of melamine, cyanuric acid and solvent is preferably: firstly, ultrasonically mixing melamine and part of the solvent to prepare a melamine solution, and ultrasonically mixing cyanuric acid and the remaining solvent to prepare a cyanuric acid solution; and then mixing the melamine solution and the cyanuric acid solution.

[0028] In the present invention, the solvent is preferably one or more of ethylene glycol, dimethyl sulfoxide, glycerol, and N,N-dimethylformamide. In the present invention, when the solvent is a mixed solvent composed of glycerol and N,N-dimethylformamide, the volume ratio of glycerol to N,N-dimethylformamide is preferably (4-8):1, more preferably 6:1. The present invention uses the above reagents as solvents to effectively regulate the micro-nano structure of the MCA supramolecular aggregate hollow spheres, and obtains MCA supramolecular aggregate hollow spheres with controllable size and complete hollow structure.

[0029] In the present invention, the concentrations of melamine and cyanuric acid in the mixed solution are preferably equal; the concentration of melamine in the mixed solution is preferably 15 to 70 mmol·L, more preferably 20 to 60 mmol·L. The present invention controls the concentrations of melamine and cyanuric acid in the mixed solution within the above range to effectively regulate the micro-nano structure of the MCA supramolecular aggregate hollow spheres, and obtains MCA supramolecular aggregate hollow spheres with controllable size and complete hollow structure.

[0030] After obtaining the mixed solution, the present invention mixes the mixed solution with a soft template agent, and sequentially performs constant temperature stirring and post-treatment to obtain MCA supramolecular aggregate hollow spheres.

[0031] In the present invention, the soft template is preferably a triblock copolymer P123. In the present invention, the mass ratio of the melamine to the soft template is preferably (3-10):1, more preferably (4-8):1, and further preferably 6:1. The present invention controls the mass ratio of melamine to the soft template within the above range to effectively regulate the micro-nano structure of the MCA supramolecular aggregate hollow sphere, and obtains the MCA supramolecular aggregate hollow sphere with controllable size and complete hollow structure.

[0032] In the present invention, the temperature of the constant temperature stirring is preferably 25 to 130°C, more preferably 30 to 120°C; the time of the constant temperature stirring is preferably 20 to 50 min, more preferably 25 to 45 min, and further preferably 30 min. In the present invention, the rate of the constant temperature stirring is preferably 300 to 800 r / min, more preferably 350 to 750 r / min. The present invention controls the temperature, time and rate of the constant temperature stirring within the above range to effectively regulate the micro-nano structure of the MCA supramolecular aggregate hollow spheres, and obtain MCA supramolecular aggregate hollow spheres with controllable size and complete hollow structure.

[0033] In the present invention, the post-treatment preferably includes: centrifugation, washing and drying in sequence.

[0034] The present invention has no special restrictions on the centrifugal method, as long as solid-liquid separation is achieved. In the present invention, the washing method is preferably alcohol washing. The present invention has no special restrictions on the alcohol washing method, as long as the residual solvent is removed. In the present invention, the drying method is preferably vacuum drying at 50-70°C for 10-16h, more preferably vacuum drying at 60°C for 12h. The present invention removes residual reagents by drying.

[0035] The invention provides a MCA supramolecular aggregate hollow sphere, which is obtained by the preparation method described in the above technical solution.

[0036] In the present invention, the MCA supramolecular aggregate hollow spheres are self-compounded by melamine and cyanuric acid through hydrogen bonds.

[0037] In the present invention, the hollow spheres of MCA supramolecular aggregates preferably have a spherical microscopic morphology with a hollow structure; the particle size of the hollow spheres of MCA supramolecular aggregates is preferably 0.7 to 8 μm, more preferably 1 to 6 μm.

[0038] The present invention also provides the use of the MCA supramolecular aggregate hollow spheres described in the above technical solution in the preparation of carbon nitride hollow sphere photocatalysts.

[0039] The method of the present invention utilizes the influence of a soft template agent to coordinately control the type of solvent, the concentration of raw materials melamine and cyanuric acid, and the temperature and time of constant temperature stirring, so as to realize the synthesis of MCA supramolecular aggregate hollow spheres with controllable particle size. The preparation method of the present invention is simple, the reaction conditions are mild, the raw materials are easily available and inexpensive, easy to control, and free of secondary pollution, which meets actual needs and is suitable for large-scale production.

[0040] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0041] Example 1

[0042] The method for preparing MCA supramolecular aggregate hollow spheres comprises the following steps:

[0043] (1) ultrasonically mixing melamine and ethylene glycol to obtain a melamine solution, ultrasonically mixing cyanuric acid and ethylene glycol to obtain a cyanuric acid solution, and mixing the melamine solution and the cyanuric acid solution at a constant temperature of 30° C. to obtain a mixed solution;

[0044] The concentration of melamine and the concentration of cyanuric acid in the mixed solution are both 20 mmol·L;

[0045] (2) adding a soft template to the mixed solution in step (2), stirring the mixture at 30° C. and 400 r / min for 30 min, and then centrifuging, washing with alcohol, and vacuum drying at 60° C. for 12 h to obtain a product, MCA supramolecular aggregate hollow spheres, which are recorded as MCA-20-30;

[0046] The mass ratio of melamine in step (1) to the soft template in step (2) is 6:1.

[0047] The MCA supramolecular aggregate hollow spheres prepared in Example 1 were detected by an X-ray diffractometer, and the X-ray diffraction pattern of the MCA supramolecular aggregate hollow spheres prepared in Example 1 was obtained as follows: Figure 1 As shown by Figure 1 It can be seen that three characteristic peaks of MCA appear at (100), (110) and (200), which confirms that melamine and cyanuric acid self-assemble in ethylene glycol solvent to form supramolecular aggregates MCA.

[0048] The MCA supramolecular aggregate hollow spheres prepared in Example 1 were detected by Fourier transform infrared spectrometer, and the Fourier transform infrared spectrum (FT-IR) of the MCA supramolecular aggregate hollow spheres prepared in Example 1 was obtained as shown in FIG. Figure 2 As shown. Figure 2 It can be seen that at 800-950cm -1 The range has characteristic peaks of hybrid aromatic rings, 1200~1750cm -1 The band at 3000-3500 cm-1 is attributed to the stretching vibration of the aromatic heterocycle, confirming the formation of the CN hybrid structure. -1 The characteristic peak at corresponds to the stacking structure of -NH2 groups, combined with Figure 1 , indicating that Example 1 successfully self-assembled and prepared MCA supramolecular aggregates.

[0049] The MCA supramolecular aggregate hollow spheres prepared in Example 1 were observed using a transmission electron microscope, and the TEM image of the MCA supramolecular aggregate hollow spheres prepared in Example 1 was obtained as shown in FIG. Figure 3 As shown. Figure 3 It can be seen that the MCA supramolecular aggregate prepared in Example 1 has a hollow sphere structure with an average particle size of 1 μm.

[0050] Example 2

[0051] MCA supramolecular aggregate hollow spheres were prepared according to the method of Example 1, except that the concentration of melamine and cyanuric acid in the mixed solution in step (1) was 40 mmol·L, and other conditions remained unchanged. The prepared product MCA supramolecular aggregate hollow spheres were denoted as MCA-40-30.

[0052] Example 3

[0053] MCA supramolecular aggregate hollow spheres were prepared according to the method of Example 1, except that the concentration of melamine and cyanuric acid in the mixed solution in step (1) was 60 mmol·L, and other conditions remained unchanged. The prepared product MCA supramolecular aggregate hollow spheres were denoted as MCA-60-30.

[0054] Example 4

[0055] MCA supramolecular aggregate hollow spheres were prepared according to the method of Example 2, except that the constant temperature stirring temperature in step (2) was 60° C., and other conditions remained unchanged. The prepared MCA supramolecular aggregate hollow spheres were denoted as MCA-40-60.

[0056] Example 5

[0057] MCA supramolecular aggregate hollow spheres were prepared according to the method of Example 2, except that the temperature of constant temperature stirring in step (2) was 100° C., and other conditions remained unchanged. The prepared product, MCA supramolecular aggregate hollow spheres, was denoted as MCA-40-100.

[0058] Example 6

[0059] MCA supramolecular aggregate hollow spheres were prepared according to the method of Example 2, except that: in step (1), a mixed solvent of glycerol and N,N-dimethylformamide in a volume ratio of 6:1 was selected as the solvent, the constant temperature stirring temperature was set to 120° C., and other conditions remained unchanged. The prepared product MCA supramolecular aggregate hollow spheres were recorded as MCA-40-120.

[0060] The MCA supramolecular aggregate hollow spheres prepared in Examples 1 to 6 were observed using a scanning electron microscope, and the SEM images of the MCA supramolecular aggregate hollow spheres prepared in Examples 1 to 6 were as follows: Figure 4 As shown, Figure 4 (a) is MCA-20-30 in Example 1, Figure 4 (b) is MCA-40-30 in Example 2, Figure 4 (c) is MCA-60-30 in Example 4, Figure 4 (d) is MCA-40-60 in Example 4, Figure 4 (e) is MCA-40-100 in Example 5, Figure 4 Wherein (f) is MCA-40-120 in Example 6. Figure 4 It can be seen that the average particle sizes of the hollow spheres of MCA supramolecular aggregates prepared in Examples 1 to 6 are 2 μm, 1.5 μm, 1 μm, 3 μm, 4.5 μm and 6 μm, respectively. It can be seen that under the same constant temperature stirring temperature conditions, the particle size of the hollow spheres of MCA supramolecular aggregates decreases with the increase of the concentration of the reactants (melamine and cyanuric acid), and under the same reactant concentration conditions, the particle size of the hollow spheres of MCA supramolecular aggregates increases with the increase of the constant temperature stirring temperature, indicating that the method provided by the present invention can effectively control the size of the product hollow spheres of MCA supramolecular aggregates by adjusting the type of solvent, the concentration of the raw materials melamine and cyanuric acid, and the constant temperature stirring temperature.

[0061] Example 7

[0062] Using the MCA supramolecular aggregate hollow spheres prepared in Example 1 as precursors, the carbon nitride hollow spheres were prepared by the supramolecular preassembly method, and the steps are as follows:

[0063] The MCA supramolecular aggregate hollow sphere solid powder prepared in Example 1 was used as a precursor, ground and put into a glass bottle, and subjected to a thermal polycondensation reaction at 550° C. in a muffle furnace, and then cooled to obtain carbon nitride hollow spheres.

[0064] The carbon nitride hollow spheres prepared in Example 7 were observed using a scanning electron microscope, and the SEM image of the carbon nitride hollow spheres prepared in Example 7 was obtained as shown in FIG. Figure 5 As shown. Figure 5 It can be seen that the average particle size of the hollow carbon nitride spheres prepared in Example 7 is 2 μm, the structure is complete, and the sphericity is high.

[0065] In summary, using the method provided by the present invention, Example 1 successfully self-assembles and prepares MCA supramolecular aggregates with an average particle size of 1 μm having a hollow sphere structure, and the MCA supramolecular aggregate hollow spheres prepared in Examples 1 to 6, under the same constant temperature stirring temperature conditions, the particle size of the product decreases with the increase of the concentration of the reactants (melamine and cyanuric acid), and under the same reactant concentration conditions, the particle size of the product increases with the increase of the constant temperature stirring temperature. By adjusting the type of solvent, the concentration of the raw materials melamine and cyanuric acid, and the constant temperature stirring temperature, the size of the product MCA supramolecular aggregate hollow spheres can be effectively controlled; Example 7 uses the MCA supramolecular aggregate hollow spheres prepared in Example 1 as a precursor, and successfully prepares carbon nitride hollow spheres with complete structure and high sphericity by using the supramolecular preassembly method. The method provided by the present invention has good application prospects in realizing controllable synthesis of carbon nitride hollow spheres by supramolecular preassembly.

[0066] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing MCA supramolecular aggregate hollow spheres, characterized in that: The following steps are involved: (1) mixing melamine, cyanuric acid and a solvent to obtain a mixed solution; (2) The mixed solution in step (2) and the soft template are mixed, and the mixture is stirred at a constant temperature and post-treated in sequence to obtain hollow spheres of MCA supramolecular aggregates.

2. The preparation method according to claim 1, characterized in that: The solvent in step (1) is one or more of ethylene glycol, dimethyl sulfoxide, propylene glycol, and N,N-dimethylformamide.

3. The preparation method according to claim 1, characterized in that: In the step (1), the concentrations of melamine and cyanuric acid in the mixed solution are equal; the concentration of melamine in the mixed solution is 15 to 70 mmol·L.

4. The preparation method according to claim 1, characterized in that: The soft template in step (2) is triblock copolymer P123.

5. The preparation method according to claim 1, characterized in that: The temperature of the constant temperature stirring in the step (2) is 25 to 130° C., and the time of the constant temperature stirring is 20 to 50 minutes.

6. The preparation method according to claim 1, characterized in that: The post-treatment in step (2) includes centrifugation, washing and drying in sequence.

7. A MCA supramolecular aggregate hollow sphere, characterized in that: The hollow spheres of MCA supramolecular aggregates are obtained by the preparation method according to any one of claims 1 to 6; the hollow spheres are self-compounded by melamine and cyanuric acid through hydrogen bonds.

8. The MCA supramolecular aggregate hollow sphere according to claim 7, characterized in that: The MCA supramolecular aggregate hollow sphere has a spherical microscopic morphology with a hollow structure and a particle size of 0.7 to 8 μm.

9. Use of the MCA supramolecular aggregate hollow spheres according to claim 7 in the preparation of carbon nitride hollow sphere photocatalysts.