Low-atomization and low-odor plasticizer for automotive interiors and preparation method of low-atomization and low-odor plasticizer
By combining epoxy fatty acid methyl ester, 2,2-dihydroxy methpropionic acid, modified polyester plasticizer, chlorinated fatty acid methyl ester and hyperbranched lignin, the prepared plasticizer is reduced during pyrolysis Atomization and odor analysis solve the problem that the existing technology of small and medium-sized molecular weight plasticizers are prone to atomization and large odor, and improve compatibility with automotive interior materials.
Patent Information
- Application Number
- CN202411252938.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the prior art, small molecular weight plasticizers such as epoxy fatty acid methyl ester have a problem of atomization and a large odor when pyrolyzed. How to reduce the atomization and analysis of automobile interior while retaining small molecular weight plasticizers. It is a technical problem that needs to be solved urgently.
By mixing 1-10 parts of epoxy fatty acid methyl ester, 10-20 parts of 2,2-dihydroxymethopropionic acid and 10-20 parts of modified polyester plasticizer, 60-80 parts of chlorine are subsequently added The fatty acid methyl ester, 20-30 parts of hyperbranched lignin and 5-10 parts of isophorone diisocyanate are naturally cooled after insulation treatment to prepare a low atomization and low odor for automobile interior decoration.
Through the reaction of hyperbranched lignin with modified polyurethane plasticizer, a migration-resistant microcrosslinking network structure is formed, which reduces the escape of epoxy fatty acid methyl ester and chlorinated fatty acid methyl ester, and significantly reduces the mist of plasticizers The chemical properties and odor improve compatibility with PP and PVC.
Smart Images

Figure BDA0005033010160000031 
Figure BDA0005033010160000032 
Figure BDA0005033010160000041
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of plasticizers, and in particular to a low-atomization and low-odor plasticizer for automobile interior decoration and a preparation method thereof. Background Art
[0002] Plasticizers are a type of additive in the plastic processing industry. Their main function is to add plastics to increase plastic shaping. Adding plasticizers to automotive interiors made of PP and PVC can weaken the van der Waals force between polymer molecular segments, increase their mobility, and reduce crystallinity, thereby increasing plastic shaping and making it easier to process.
[0003] Common plasticizers include dioctyl phthalate, dibutyl phthalate, etc. However, with the introduction of the green environmental protection concept, people have gradually abandoned such plasticizers that pollute the environment and harm the human body. Environmentally friendly polyester and epoxy vegetable oil plasticizers have gradually developed, especially polyester plasticizers due to their high molecular weight and good compatibility with PVC and PP. They are widely used in automotive interior materials. In addition, small molecular weight chloromethyl fatty acid esters and other ingredients have a strong odor and are easy to atomize during pyrolysis.
[0004] Patent application CN113801484A discloses a low-odor, non-toxic, non-benzene, environmentally friendly composite plasticizer. The composite plasticizer is prepared by mixing diisononyl 1,2-cyclohexanedicarboxylate, winterized epoxy palm oil, winterized epoxy palm oil methyl ester, phosphite, calcium ricinoleate and zinc ricinoleate. The unepoxidized saturated oil or saturated fatty acid methyl ester portion with a stronger odor in the epoxy oil ester and the epoxy fatty acid methyl ester is removed through a winterization process, so that the prepared plasticizer has the characteristic of low odor. However, winterization of the epoxy fatty acid methyl ester in advance will result in the removal and waste of small molecular plasticizers. How to reduce the fogging and precipitation phenomenon of automotive interiors while retaining small molecular weight plasticizers is a technical problem that needs to be solved urgently. Summary of the invention
[0005] The purpose of the present invention is to provide a method for preparing a plasticizer with low atomization and low odor for automobile interior decoration, which is used to solve the technical problem that small molecular weight plasticizers such as epoxy fatty acid methyl ester in the prior art are easy to atomize and have a strong odor during pyrolysis.
[0006] The purpose of the present invention can be achieved by the following technical scheme: A method for preparing a low-atomization and low-odor plasticizer for automobile interior decoration, comprising the following steps:
[0007] S1. Mix 1-10 parts of epoxy fatty acid methyl ester, 10-20 parts of 2,2-dihydroxymethacrylic acid and 10-20 parts of modified polyester plasticizer by weight, and keep warm at 90-100° C. for 30 minutes to obtain a mixture;
[0008] S2. According to parts by weight, 60-80 parts of chloro fatty acid methyl ester, 20-30 parts of hyperbranched lignin and 5-10 parts of isophorone diisocyanate are added to the mixture, and the mixture is kept warm at 70-75° C. for 30-60 minutes to obtain a product; the product is naturally cooled to room temperature to obtain a low-fogging and low-odor plasticizer for automotive interior.
[0009] Furthermore, the preparation method of the modified polyester plasticizer comprises the following steps:
[0010] A1, 1,9-sebanic acid and 1,2-butanediol were mixed and subjected to esterification reaction at 180°C in a nitrogen atmosphere until no water was refluxed, then stannous chloride was added, the temperature was raised to 250°C and the reaction was continued for 2-3h, then the excess 1,2-butanediol was distilled under reduced pressure and the stannous chloride was filtered out to obtain intermediate A;
[0011] A2, intermediate A and epoxidized soybean oil are mixed and reacted at 130-140° C. for 1-2 hours to obtain a modified polyurethane plasticizer.
[0012] 1,9-Sebacic acid and 1,2-butanediol are used as raw materials, and after esterification and polycondensation reactions, an oligomeric polyester plasticizer is obtained. The terminal hydroxyl group of the oligomeric polyester plasticizer can react with the epoxy group of epoxidized soybean oil to obtain a modified polyester plasticizer.
[0013] Furthermore, in step A1, the usage ratio of 1,9-sebanic acid, 1,2-butanediol and stannous chloride is 15g:20-30g:0.2g; in step A2, the usage of epoxidized soybean oil is 10-20g.
[0014] The low-fogging and low-odor plasticizer for automobile interior decoration prepared by the present invention is prepared by using epoxy fatty acid methyl ester and chloro fatty acid methyl ester as auxiliary plasticizers, 2,2-dihydroxymethacrylic acid as a cosolvent, isophorone diisocyanate as a cross-linking curing agent, modified polyester plasticizer as a small molecule plasticizer, and hyperbranched lignin as a macromolecular plasticizer.
[0015] Furthermore, the preparation method of the hyperbranched lignin comprises the following steps:
[0016] B1, phenolic lignin, toluene and 3-mercaptopropyl-3-methoxysilane are mixed, and refluxed at 90-100° C. for 48 hours to obtain a mixed solid-liquid; the mixed solid-liquid is subjected to post-processing to obtain modified lignin;
[0017] Lignin is a polyhydroxy aromatic compound containing multiple functional groups such as alcoholic hydroxyl, phenolic hydroxyl, carboxyl, etc. Lignin is pre-treated with phenol, and the para-position or ortho-position of phenol is connected to lignin in the form of a carbon-carbon bond to obtain phenolated lignin with an increased hydroxyl content. Toluene is used as a solvent, and the hydroxyl groups on the surface of lignin and the silicon-oxygen bonds in 3-mercaptopropyl-3-methoxysilane are reacted and dehydrated to prepare modified lignin containing mercapto groups.
[0018] The reaction formula for synthesizing modified lignin from phenolized lignin and 3-mercaptopropyl-3-methoxysilane is as follows:
[0019]
[0020] B2, cyanuric chloride, anhydrous sodium carbonate and 1,4-dioxane are uniformly mixed to obtain a reaction mixture; ethylenediamine is added dropwise to the reaction mixture, first reacted at 0-10°C for 3 hours, and then reacted at a constant temperature of 50°C for 3 hours to obtain a product; the product is filtered, washed with deionized water, and dried to obtain a branched cyanuric chloride solid;
[0021] With 1,4-dioxane as solvent and anhydrous sodium carbonate as catalyst, cyanuric chloride and ethylenediamine undergo nucleophilic substitution reaction to prepare branched cyanuric chloride solid.
[0022] The reaction formula for the generation of branched cyanuric chloride from cyanuric chloride and ethylenediamine is as follows:
[0023]
[0024] B3. The modified lignin, branched cyanuric chloride and toluene are mixed and reacted at 50-60° C. for 3-4 hours to obtain a product; the product is filtered and washed with deionized water to obtain hyperbranched lignin.
[0025] Using toluene as solvent, the thiol functional groups on the surface of modified lignin and the amino groups and chloride ions in branched cyanuric chloride can undergo nucleophilic substitution reactions to prepare hyperbranched lignin.
[0026] The reaction formula for synthesizing hyperbranched lignin by reacting modified lignin with branched cyanuric chloride is as follows:
[0027]
[0028] Furthermore, in step B1, the method for preparing phenolic lignin comprises the following steps:
[0029] 100-200 g of lignin, 100 g of phenol and 5 mL of 5% wt H2SO4 solution are mixed evenly, and reacted at 100-120° C. for 2-2.5 hours to obtain a mixed solution; 100 mL of deionized water is added to the mixed solution, stirred for 10-20 minutes, and then allowed to stand and precipitate, and a solid is obtained by filtration; the solid is washed three times with deionized water, and then vacuum dried at 30-40° C. to constant weight to obtain phenolic lignin.
[0030] Furthermore, in step B1, the usage ratio of phenolized lignin, toluene and 3-mercaptopropyl-3-methoxysilane is 30g:100mL:10-20g; the post-process steps include: filtering and centrifuging the mixed solid-liquid to obtain a solid, washing the solid with deionized water to remove the toluene solvent, and vacuum drying at 60°C to constant weight to obtain modified lignin.
[0031] Furthermore, in step B2, the usage ratio of cyanuric chloride, anhydrous sodium carbonate, 1,4-dioxane and ethylenediamine is 30g:20g:400mL:12-18g; in step B3, the usage ratio of modified lignin, chemical cyanuric chloride and toluene is 30g:30-40g:200mL.
[0032] As another aspect of the present invention, a method for preparing a low-fogging and low-odor plasticizer for automobile interior is provided to prepare the low-fogging and low-odor plasticizer for automobile interior.
[0033] The present invention has the following beneficial effects:
[0034] 1. Lignin is pre-phenolized with phenol to increase the hydroxyl content of lignin itself to obtain phenolized lignin, and phenolized lignin is grafted with 3-mercaptopropyl-3-methoxysilane to introduce mercapto functional groups to obtain modified lignin; cyanuric chloride contains polychloride ions and can react with ethylenediamine to obtain branched cyanuric chloride containing polychloride ions and polyamino groups; the mercapto groups in the modified lignin can react with the functional groups in the branched cyanuric chloride, so that cyanuric chloride is used as an intermediate to polymerize lignin units to obtain hyperbranched lignin. The hyperbranched lignin is used as a macromolecular plasticizer, and the hydroxyl group, carboxyl group, amino group and chloride ion contained in the hyperbranched lignin can react with the epoxy group in the modified polyurethane plasticizer, so as to attract and fix the modified polyurethane plasticizer with a small molecular weight, inhibit the precipitation of the plasticizer, and thus prepare a plasticizer with low atomization properties; the present invention uses 1,9-seedioic acid and 1,2-butanediol to synthesize oligomers, adds a certain amount of epoxy soybean oil for modification, and the prepared modified polyurethane plasticizer has the advantage of being completely biodegradable; in addition, the selected polyurethane plasticizer itself has excellent compatibility with PP resin and PVC resin used for automobile interior decoration.
[0035] 2. The present invention uses epoxy fatty acid methyl ester and chloro fatty acid methyl ester as auxiliary plasticizers to construct a continuous phase of the plasticizer; chloro fatty acid methyl ester, as a common plasticizer component, decomposes by heating to produce toxic chlorides and smelly and irritating organic small molecule compounds, so that the prepared plasticizer produces a strong odor during specific use; epoxy fatty acid methyl ester, as a small molecular weight organic substance, has poor stability itself; by adding hyperbranched lignin and cross-linking agent isophorone diisocyanate, the prepared plasticizer forms a migration-resistant micro-cross-linked network structure when compatible with PP and PC, thereby reducing the escape of epoxy fatty acid methyl ester and chloro fatty acid methyl ester, and preparing a low-odor modified polyester plasticizer. DETAILED DESCRIPTION
[0036] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0037] Example 1
[0038] This embodiment provides a method for preparing a modified polyester plasticizer for a low-atomization and low-odor plasticizer for automobile interior decoration, comprising the following steps:
[0039] A1. A 250 mL four-necked flask is connected with a magnetic stirrer, a thermometer, a nitrogen tube and a water separator in sequence, and the upper end of the water separator is connected with a reflux condenser; 15 g of 1,9-conigaoic acid and 20 g of 1,2-butanediol are added to the four-necked flask, and the four-necked flask is heated by an electric heating jacket, and the heating temperature is set to 180°C; nitrogen is filled into the four-necked flask through the nitrogen tube, and an esterification reaction is carried out under nitrogen protection until there is no water in the reflux, and then 0.2 g of catalyst stannous chloride is added, and the four-necked flask is heated to 250°C and the reflux reaction is continued for 2 hours, and finally the excess 1,2-butanediol is distilled off under reduced pressure, and the catalyst stannous chloride is filtered out with a Buchner funnel to obtain a liquid intermediate A.
[0040] A2. Add all the liquid intermediate A into a 250 mL four-necked flask, and then add
[0041] 10 g of epoxidized soybean oil was reacted in a four-necked flask at 130° C. for 1 h accompanied by mechanical stirring at 100 r / min to obtain a modified polyurethane plasticizer.
[0042] Example 2
[0043] This embodiment provides a method for preparing a modified polyester plasticizer for a low-atomization and low-odor plasticizer for automobile interior decoration, comprising the following steps:
[0044] A1. A 250 mL four-necked flask is connected with a magnetic stirrer, a thermometer, a nitrogen tube and a water separator in sequence, and the upper end of the water separator is connected with a reflux condenser; 15 g of 1,9-seedanoic acid and 25 g of 1,2-butanediol are added to the four-necked flask, and the four-necked flask is heated by an electric heating jacket, and the heating temperature is set to 180°C; nitrogen is filled into the four-necked flask through the nitrogen tube, and an esterification reaction is carried out under nitrogen protection until there is no water in the reflux, and then 0.2 g of a catalyst stannous chloride is added, and the four-necked flask is heated to 250°C and the reflux reaction is continued for 2.3 hours, and finally the excess 1,2-butanediol is distilled off under reduced pressure, and the catalyst stannous chloride is filtered out with a Buchner funnel to obtain a liquid intermediate A.
[0045] A2. Add all the liquid intermediate A into a 250 mL four-necked flask, and then add
[0046] 15 g of epoxidized soybean oil was reacted in a four-necked flask at 130° C. for 1 h accompanied by mechanical stirring at 100 r / min to obtain a modified polyurethane plasticizer.
[0047] Example 3
[0048] This embodiment provides a method for preparing a modified polyester plasticizer for a low-atomization and low-odor plasticizer for automobile interior decoration, comprising the following steps:
[0049] A1. A 250 mL four-necked flask is connected with a magnetic stirrer, a thermometer, a nitrogen tube and a water separator in sequence, and the upper end of the water separator is connected with a reflux condenser; 15 g of 1,9-seedanoic acid and 30 g of 1,2-butanediol are added to the four-necked flask, and the four-necked flask is heated by an electric heating jacket, and the heating temperature is set to 180° C.; nitrogen is filled into the four-necked flask through a nitrogen tube, and an esterification reaction is carried out under nitrogen protection until there is no water in the reflux, and then 0.2 g of a catalyst stannous chloride is added, and the four-necked flask is heated to 250° C. and the reflux reaction is continued for 3 hours, and finally the excess 1,2-butanediol is distilled off under reduced pressure, and the catalyst stannous chloride is filtered out with a Buchner funnel to obtain a liquid intermediate A.
[0050] A2. Add all the liquid intermediate A into a 250 mL four-necked flask, and then add
[0051] 20 g of epoxidized soybean oil was reacted in a four-necked flask at 130° C. for 1 h accompanied by mechanical stirring at 100 r / min to obtain a modified polyurethane plasticizer.
[0052] Example 4
[0053] This embodiment provides a method for preparing hyperbranched lignin for a plasticizer with low atomization and low odor for automobile interior decoration, comprising the following steps:
[0054] B1. Add 100g of lignin and 100g of phenol to a 500mL hydrothermal reactor, add 5mL of 5%wt H2SO4 solution, mix and stir at 200r / min for 5min to obtain a premixed solution; then heat the hydrothermal reactor to 100°C, react for 2h, and after the reaction is completed, cool to room temperature to obtain a mixed solution; add 100mL of deionized water to the mixed solution, stir at 200r / min for 10min, then let it stand and precipitate, and filter to obtain a solid. The solid is washed three times with deionized water, and vacuum dried at 70°C to constant weight to obtain phenolic lignin.
[0055] B2. Weigh 30 g of phenolized lignin and 100 mL of toluene and add them to a 250 mL three-necked flask, then add 10 g of 3-mercaptopropyl-3-methoxysilane to the three-necked flask, transfer the three-necked flask to a water bath, reflux at 90 ° C for 48 hours to obtain a mixed solid-liquid; the mixed solid-liquid is filtered and centrifuged to obtain a solid; the solid is washed with deionized water for several times to remove the toluene solvent, and vacuum dried at 60 ° C to constant weight to obtain modified lignin.
[0056] B3. A separatory funnel is set in a 1000mL three-necked flask, and 30g of cyanuric chloride, 20g of anhydrous sodium carbonate and 400mL of 1,4-dioxane are added into the three-necked flask, and mixed evenly to obtain a reaction mixture; 12g of ethylenediamine is added dropwise into the three-necked flask through the separatory funnel; the three-necked flask is transferred to a water bath, and the three-necked flask is first reacted at 0°C for 3h, and then the temperature of the water bath is adjusted to 50°C, and the reaction is carried out at a constant temperature for 3h to obtain a product; the product is filtered, washed with deionized water, and dried to obtain a branched cyanuric chloride solid.
[0057] B4. Add 30 g of modified lignin, 34 g of branched cyanuric chloride and 200 mL of toluene into a 500 mL beaker, transfer the beaker to a water bath, set the temperature of the water bath to 56 ° C, and react for 3.3 hours with mechanical stirring at 100 r / min to obtain a product; filter the product and wash with deionized water to obtain hyperbranched lignin.
[0058] Example 5
[0059] This embodiment provides a method for preparing hyperbranched lignin for a plasticizer with low atomization and low odor for automobile interior decoration, comprising the following steps:
[0060] B1. Add 200g of lignin and 100g of phenol to a 500mL hydrothermal reactor, add 5mL of 5%wt H2SO4 solution, mix and stir at 200r / min for 6min to obtain a premixed solution; then heat the hydrothermal reactor to 110°C, react for 2.2h, and after the reaction is completed, cool to room temperature to obtain a mixed solution; add 100mL of deionized water to the mixed solution, stir at 200r / min for 15min, then let it stand and precipitate, and filter to obtain a solid. The solid is washed three times with deionized water, and vacuum dried at 75°C to constant weight to obtain phenolic lignin.
[0061] B2. Weigh 30 g of phenolized lignin and 100 mL of toluene and add them to a 250 mL three-necked flask, then add 17 g of 3-mercaptopropyl-3-methoxysilane to the three-necked flask, transfer the three-necked flask to a water bath, and reflux at 92 ° C for 48 hours to obtain a mixed solid-liquid; the mixed solid-liquid is filtered and centrifuged to obtain a solid; the solid is washed with deionized water for several times to remove the toluene solvent, and vacuum dried at 60 ° C to constant weight to obtain modified lignin.
[0062] B3. A separatory funnel is set in a 1000mL three-necked flask, and 30g of cyanuric chloride, 20g of anhydrous sodium carbonate and 400mL of 1,4-dioxane are added into the three-necked flask, and mixed evenly to obtain a reaction mixture; 15g of ethylenediamine is added dropwise into the three-necked flask through the separatory funnel; the three-necked flask is transferred to a water bath, and the three-necked flask is first reacted at 3°C for 3h, and then the temperature of the water bath is adjusted to 50°C, and the reaction is carried out at a constant temperature for 3h to obtain a product; the product is filtered, washed with deionized water, and dried to obtain a branched cyanuric chloride solid.
[0063] B4. Add 30 g of modified lignin, 32 g of branched cyanuric chloride and 200 mL of toluene into a 500 mL beaker, transfer the beaker to a water bath, set the temperature of the water bath to 58 ° C, and react for 3.3 hours with mechanical stirring at 100 r / min to obtain a product; filter the product and wash with deionized water to obtain hyperbranched lignin.
[0064] Example 6
[0065] This embodiment provides a method for preparing hyperbranched lignin for a plasticizer with low atomization and low odor for automobile interior decoration, comprising the following steps:
[0066] B1. Add 200g of lignin and 100g of phenol to a 500mL hydrothermal reactor, add 5mL of 5%wt H2SO4 solution, mix and stir at 200r / min for 10min to obtain a premixed solution; then heat the hydrothermal reactor to 120°C, react for 2.5h, and after the reaction is completed, cool to room temperature to obtain a mixed solution; add 100mL of deionized water to the mixed solution, stir at 200r / min for 20min, then let it stand and precipitate, and filter to obtain a solid. The solid is washed three times with deionized water, and then vacuum dried at 80°C to constant weight to obtain phenolic lignin.
[0067] B2. Weigh 30 g of phenolized lignin and 100 mL of toluene and add them to a 250 mL three-necked flask, then add 20 g of 3-mercaptopropyl-3-methoxysilane to the three-necked flask, transfer the three-necked flask to a water bath, and reflux at 100 ° C for 48 hours to obtain a mixed solid-liquid; the mixed solid-liquid is filtered and centrifuged to obtain a solid; the solid is washed with deionized water for several times to remove the toluene solvent, and vacuum dried at 60 ° C to constant weight to obtain modified lignin.
[0068] B3. A separatory funnel is set in a 1000mL three-necked flask, and 30g of cyanuric chloride, 20g of anhydrous sodium carbonate and 400mL of 1,4-dioxane are added into the three-necked flask, and mixed evenly to obtain a reaction mixture; 18g of ethylenediamine is added dropwise into the three-necked flask through the separatory funnel; the three-necked flask is transferred to a water bath, and the three-necked flask is first reacted at 10°C for 3h, and then the temperature of the water bath is adjusted to 50°C, and the reaction is carried out at a constant temperature for 3h to obtain a product; the product is filtered, washed with deionized water, and dried to obtain a branched cyanuric chloride solid.
[0069] B4. Add 30 g of modified lignin, 40 g of branched cyanuric chloride and 200 mL of toluene into a 500 mL beaker, transfer the beaker to a water bath, set the temperature of the water bath to 60 ° C, and react for 4 hours with mechanical stirring at 100 r / min to obtain a product; filter the product and wash with deionized water to obtain hyperbranched lignin.
[0070] Example 7
[0071] This embodiment provides a method for preparing a low-atomization and low-odor plasticizer for automobile interior decoration, comprising the following steps:
[0072] S1. In a 250 mL three-necked flask, 1 part of epoxy fatty acid methyl ester, 10 parts of 2,2-dihydroxymethacrylic acid and 10 parts of the modified polyester plasticizer prepared in Example 1 were added, according to parts by weight. The three-necked flask was transferred to a water bath, the temperature of the water bath was set to 90° C., and stirred at 100 r / min for 30 min at this temperature to obtain a mixture.
[0073] S2, according to weight parts, add 60 parts of chloro fatty acid methyl ester, 20 parts of hyperbranched lignin prepared in Example 4 and 5 parts of isophorone diisocyanate to the three-necked flask, adjust the temperature of the water bath to 70 ° C, accompanied by mechanical stirring at 100 r / min, and keep the water bath at this temperature for 30 minutes to obtain a product. The product is naturally cooled to room temperature to prepare a plasticizer with low atomization and low odor for automotive interior.
[0074] Example 8
[0075] This embodiment provides a method for preparing a low-atomization and low-odor plasticizer for automobile interior decoration, comprising the following steps:
[0076] S1. In a 250 mL three-necked flask, 5 parts of epoxy fatty acid methyl ester, 15 parts of 2,2-dihydroxymethacrylic acid and 15 parts of the modified polyester plasticizer prepared in Example 2 were added, according to parts by weight, and the three-necked flask was transferred to a water bath, the temperature of the water bath was set to 95° C., and stirred at 110 r / min for 30 min at this temperature to obtain a mixture.
[0077] S2, according to weight parts, add 70 parts of chloro fatty acid methyl ester, 26 parts of hyperbranched lignin prepared in Example 5 and 6 parts of isophorone diisocyanate to the three-necked flask, adjust the temperature of the water bath to 72 ° C, accompanied by mechanical stirring at 100r / min, and keep the water bath at this temperature for 40min to obtain a product. The product is naturally cooled to room temperature to prepare a low-fogging and low-odor plasticizer for automotive interior.
[0078] Example 9
[0079] This embodiment provides a method for preparing a low-atomization and low-odor plasticizer for automobile interior decoration, comprising the following steps:
[0080] S1. In a 250 mL three-necked flask, 10 parts of epoxy fatty acid methyl ester, 20 parts of 2,2-dihydroxymethacrylic acid and 20 parts of the modified polyester plasticizer prepared in Example 3 were added, according to parts by weight, and the three-necked flask was transferred to a water bath, the temperature of the water bath was set to 100° C., and stirred at 120 r / min for 30 min at this temperature to obtain a mixture.
[0081] S2, according to weight parts, add 80 parts of chloro fatty acid methyl ester, 30 parts of hyperbranched lignin prepared in Example 6 and 10 parts of isophorone diisocyanate to the three-necked flask, adjust the temperature of the water bath to 75 ° C, accompanied by mechanical stirring at 100r / min, and keep the water bath at this temperature for 60min to obtain a product. The product is naturally cooled to room temperature to prepare a plasticizer with low atomization and low odor for automotive interior.
[0082] Comparative Example 1
[0083] The difference between this comparative example and Example 9 is that when preparing the modified polyester plasticizer, no epoxy soybean oil is added, and the liquid intermediate A is the modified polyester plasticizer.
[0084] Comparative Example 2
[0085] The difference between this comparative example and Example 9 is that cyanuric chloride is not reacted with ethylenediamine to prepare branched cyanuric chloride.
[0086] Comparative Example 3
[0087] The difference between this comparative example and Example 9 is that the hyperbranched lignin is replaced by modified lignin.
[0088] Performance test 1:
[0089] 1. According to GB / T1668-2008 "Determination of Acid Value and Acidity of Plasticizers", the acid values of the low-fogging and low-odor plasticizers for automotive interiors prepared in Examples 7-9 and Comparative Examples 1-3 were measured. Each group was measured three times, and the final result was the average of the three tests.
[0090] 2. The viscosity of the low-fogging and low-odor plasticizers for automotive interiors prepared in Examples 7-9 and Comparative Example 1 was measured using a rotary viscometer. The test was conducted at room temperature of 25°C, and the rotor used was S63. The reading was taken after the viscosity reading stabilized, which was the viscosity of the sample to be tested. The specific test results are shown in Table 1.
[0091] Table 1 - Performance test data table
[0092]
[0093] Data Analysis:
[0094] The low-fogging and low-odor plasticizers for automotive interiors prepared in Examples 7-9 of the present invention all have lower acid values, indicating that when 1,9-seedioic acid and 1,2-butanediol are used to prepare the modified polyurethane plasticizer, the esterification is complete and the esterification reaction is considered to have reached the endpoint; the low-fogging and low-odor plasticizers for automotive interiors prepared in Examples 7-9 of the present invention all have suitable viscosity values. In Comparative Example 1, epoxy soybean oil was not added when preparing the modified polyurethane plasticizer, which slightly reduced the viscosity value of the prepared plasticizer. However, the viscosity values of the plasticizers prepared in Examples 7-9 and Comparative Example 1 were both within the easy processing range.
[0095] Performance Test 2:
[0096] The low-fogging and low-odor plasticizers for automotive interior prepared in Examples 7-9 and Comparative Examples 2-3 were sequentially mixed with calcium / zinc heat stabilizers and PVC powder according to a proportion, placed in a high-speed mechanical stirrer and stirred for 5 minutes. After the materials were evenly mixed, the temperature of the open mill was set to 160°C, the roller spacing was 0.8 cm, and the rotation speed was 50 r / min to obtain a mixed material; the mixed material was added to the open mill and plasticized for 10 minutes, and then the mixed material was placed in a mold and placed in a flat-plate vulcanizer for tableting to obtain a PVC test piece; the PVC test piece was placed in a mold, placed in an automatic flat-plate vulcanizer for tableting, and the material was discharged after hot pressing and cold pressing. The prepared sheet PVC was cut into dumbbell-shaped strips of the same size with a cutter to obtain a plasticizer product, which was marked as Examples 8-12 and Comparative Examples 4-5 in turn.
[0097] 3. The plasticizer products prepared in Examples 10-12 and Comparative Examples 4-5 were subjected to thermogravimetric analysis using a TG209-C thermogravimetric analyzer to determine the temperature corresponding to a weight loss rate of 30%. During the experiment, nitrogen atmosphere was used for inlet air, the heating rate was set to 10°C / min, and the temperature range was 40-600°C.
[0098] 4. According to GB / T1040.3-2006 "Determination of tensile properties of plastics", the tensile strength and elongation at break of the plasticizer products prepared in Examples 7-9 and Comparative Examples 1-3 were tested.
[0099] 5. According to the "ISO176-2005 activated carbon adsorption method", the migration resistance of the plasticizer products prepared in Examples 10-12 and Comparative Examples 4-5 was tested after being placed in an oven at 100°C for 8 hours; each sample was tested 3 times, and the mass loss rate was calculated as the average of the 3 experimental data. The specific test results are shown in the following table:
[0100] Table 2 - Performance test data table
[0101]
[0102] Data Analysis:
[0103] By comparing and analyzing the data in the above table, the plasticizer products prepared in Examples 10-12 of the present invention all have high thermal stability, which is specifically manifested in that when the weight loss rate is 30%, the temperature of the plasticizer products prepared in Examples 10-12 is relatively high; the plasticizer products prepared in Examples 10-12 of the present invention all have excellent mechanical properties, which is manifested in that the plasticizer products prepared in Examples 10-12 all have high tensile strength values and elongation at break values; however, when preparing the plasticizer in Comparative Example 2, cyanuric chloride is not modified with ethylenediamine; when preparing the plasticizer in Comparative Example 3, the modified lignin is not modified with cyanuric chloride, and hyperbranched lignin is synthesized, so that the mechanical properties of the plasticizer products prepared in Comparative Examples 4 and 5 are reduced, the thermal stability is reduced, and the mobility is increased.
[0104] The above contents are merely examples and explanations of the structure of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the structure of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.
[0105] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0106] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to only specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A method for preparing a low-atomization and low-odor plasticizer for automobile interior decoration, It is characterized in that The following steps are involved: S1. Mix 1-10 parts of epoxy fatty acid methyl ester, 10-20 parts of 2,2-dihydroxymethacrylic acid and 10-20 parts of modified polyester plasticizer by weight, and keep warm at 90-100° C. for 30 minutes to obtain a mixture; S2. According to parts by weight, 60-80 parts of chloro fatty acid methyl ester, 20-30 parts of hyperbranched lignin and 5-10 parts of isophorone diisocyanate are added to the mixture, and the mixture is kept warm at 70-75° C. for 30-60 minutes to obtain a product; the product is naturally cooled to room temperature to obtain a low-fogging and low-odor plasticizer for automotive interior.
2. A method for preparing a low-atomization and low-odor plasticizer for automobile interior according to claim 1, It is characterized in that The preparation method of the modified polyester plasticizer comprises the following steps: A1, 1,9-sebanic acid and 1,2-butanediol were mixed and subjected to esterification reaction at 180°C in a nitrogen atmosphere until no water was refluxed, then stannous chloride was added, the temperature was raised to 250°C and the reaction was continued for 2-3h, then the excess 1,2-butanediol was distilled under reduced pressure and the stannous chloride was filtered out to obtain intermediate A; A2, intermediate A and epoxidized soybean oil are mixed and reacted at 130-140° C. for 1-2 hours to obtain a modified polyurethane plasticizer.
3. A method for preparing a low-atomization and low-odor plasticizer for automobile interior according to claim 2, It is characterized in that In step A1, the usage ratio of 1,9-sebanic acid, 1,2-butanediol and stannous chloride is 15g:20-30g:0.2g; in step A2, the usage of epoxidized soybean oil is 10-20g.
4. The method for preparing the low-fogging and low-odor plasticizer for automobile interior according to claim 1, It is characterized in that The preparation method of the hyperbranched lignin comprises the following steps: B1, phenolic lignin, toluene and 3-mercaptopropyl-3-methoxysilane are mixed, and refluxed at 90-100° C. for 48 hours to obtain a mixed solid-liquid; the mixed solid-liquid is subjected to post-processing to obtain modified lignin; B2, cyanuric chloride, anhydrous sodium carbonate and 1,4-dioxane are uniformly mixed to obtain a reaction mixture; ethylenediamine is added dropwise to the reaction mixture, first reacted at 0-10°C for 3 hours, and then reacted at a constant temperature of 50°C for 3 hours to obtain a product; the product is filtered, washed with deionized water, and dried to obtain solid branched cyanuric chloride; B3. The modified lignin, branched cyanuric chloride and toluene are mixed and reacted at 50-60° C. for 3-4 hours to obtain a product; the product is filtered and washed with deionized water to obtain hyperbranched lignin.
5. A method for preparing a low-atomization and low-odor plasticizer for automobile interior according to claim 4, It is characterized in that In step B1, the method for preparing phenolic lignin comprises the following steps: 100-200g of lignin, 100g of phenol and 5%wt of H 2 SO 4 5 mL of the solution was mixed evenly, and reacted at 100-120° C. for 2-2.5 hours to obtain a mixed solution; 100 mL of deionized water was added to the mixed solution, stirred for 10-20 minutes, and then allowed to stand and precipitate, and a solid was obtained by filtration; the solid was washed three times with deionized water, and then vacuum dried at 70-80° C. to constant weight to obtain phenolic lignin.
6. A method for preparing a low-fogging and low-odor plasticizer for automobile interior according to claim 5, It is characterized in that In step B1, the ratio of phenolic lignin, toluene and 3-mercaptopropyl-3-methoxysilane is 30 g:100 mL:10-20 g; The post-process steps include: filtering and centrifuging the mixed solid and liquid to obtain a solid, washing the solid with deionized water to remove the toluene solvent, and vacuum drying at 60° C. to a constant weight to obtain modified lignin.
7. A method for preparing a low-fogging and low-odor plasticizer for automobile interior according to claim 6, It is characterized in that In step B2, the usage ratio of cyanuric chloride, anhydrous sodium carbonate, 1,4-dioxane and ethylenediamine is 30g:20g:400mL:12-18g; in step B3, the usage ratio of modified lignin, branched cyanuric chloride and toluene is 30g:30-40g:200mL.
8. A low-fogging and low-odor plasticizer for automotive interiors. It is characterized in that The plasticizer is prepared by the method for preparing a low-atomization and low-odor plasticizer for automobile interior decoration as described in any one of claims 1 to 7.
Citation Information
Patent Citations
Migration-resistant environment-friendly plasticizer with micro-crosslinking structure and preparation method of same
CN113402891A
Low-fogging-degree environment-friendly plasticizer
CN114790162A
Cited By
Plasticizer capable of reducing viscosity at low temperature and preparation method thereof
CN121108580A