Hexagonal boron nitride composite material and preparation method thereof

By treating with surfactants and magnetizing to form a core-shell structure, hexagonal boron nitride composite material was formed, which solved the problems of uneven filler dispersion and orientation, and achieved high efficiency in thermal conductivity and insulation performance, making it suitable for thermal management of electronic devices.

CN118994904APending Publication Date: 2024-11-22SHANGHAI MARITIME UNIVERSITY
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411204103.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In existing technologies, uneven dispersion and agglomeration of fillers in polymer composites result in limited improvement in thermal conductivity. Mechanical molding affects the integrity and orientation of two-dimensional fillers, making it difficult to form efficient thermal conduction paths.

Method used

Hexagonal boron nitride is treated with surfactants and then magnetically treated to form a core-shell structure. Hexagonal boron nitride particles are oriented in a resin matrix using magnetic materials, and their orientation is controlled by a magnetic field to form an efficient heat conduction path.

Benefits of technology

It significantly improves the dispersibility and orientation of fillers, enhances the thermal conductivity and insulation properties of electronic components, and improves the heat dissipation capacity of composite materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994904A_ABST
    Figure CN118994904A_ABST
Patent Text Reader

Abstract

The invention discloses a hexagonal boron nitride composite material and a preparation method thereof, the material comprises a resin matrix and core-shell particles directionally distributed in the resin matrix, the core of each core-shell particle is a surfactant modified hexagonal boron nitride, and the shell is a magnetic material. The core-shell type structure can improve the dispersibility and orientation of the filler, can obviously improve the heat dissipation capability of electronic components, can effectively improve the insulating property of the composite material, enables the composite material to have excellent power transmission performance, and has great application potential in heat-conducting composite materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to electronic equipment materials and a preparation method thereof, and in particular to a hexagonal boron nitride composite material and a preparation method thereof. Background Art

[0002] With the advent of the 5G era, electronic devices are developing rapidly towards higher integration and more functions. Electronic devices will generate a lot of heat inside the device when working at high power. If the heat cannot be conducted out in time, it will cause safety hazards to the equipment. According to statistics, 55% of electronic equipment failures are caused by temperatures exceeding the allowable value, so the thermal management performance of electronic devices is one of the important factors restricting its development. At present, the common method to improve the thermal conductivity of polymers is fillers such as carbon fiber, boron nitride, and graphene, but the uneven dispersion of fillers in the matrix and the formation of agglomeration are the main reasons for the small improvement in the thermal conductivity of composite materials. The polymer is mixed with the two-dimensional filler, and then sintered after pulse vibration molding to obtain a high thermal conductivity polymer composite material, enhance the deformation ability of the polymer, improve the orientation of the two-dimensional filler, and the interface thermal conductivity path, so that the composite material has stronger thermal conductivity. However, the use of mechanical means to mold will affect the integrity and orientation of the two-dimensional filler. In order to form a high-quality thermal conductivity path inside the composite material, it is an effective method to use non-mechanical means to orient the two-dimensional filler. Summary of the invention

[0003] Purpose of the invention: The present invention provides a hexagonal boron nitride composite material and a preparation method thereof, wherein the composite material can improve the dispersion and orientation of fillers and enhance the thermal conductivity of electronic components.

[0004] Technical solution: The first aspect of the present invention provides the hexagonal boron nitride composite material, comprising a resin matrix and core-shell particles directionally distributed in the resin matrix, wherein the core of the core-shell particle is surfactant-modified hexagonal boron nitride, and the shell is a magnetic material.

[0005] A second aspect of the present invention provides a thermally conductive composite material, which is prepared using the hexagonal boron nitride composite material according to claim 1.

[0006] The third aspect of the present invention provides a method for preparing the hexagonal boron nitride composite material, comprising the following steps:

[0007] (1) adding a hydrochloric acid solution to a surfactant solution, and then adding hexagonal boron nitride to adjust the pH value of the solution;

[0008] (2) Add FeCl3 solution and FeCl2 solution to the mixed solution of step (1) to achieve Fe 3+ with Fe 2+The molar ratio of is controlled at 2:1, sodium hydroxide solution and ammonia solution are added, and then 1,6-hexanediamine solution is added to the mixture, and the mixture is filtered and washed three times with deionized water to remove excess amine molecules, and dried to obtain a hexagonal boron nitride material with magnetic activity;

[0009] (3) Magnetic treatment: adding a resin matrix to the material obtained in step (2) to perform magnetic treatment, and after the magnetic treatment, continuing to increase the magnetic induction intensity, and controlling the direction of the magnetic field to be in the vertical direction;

[0010] (4) Curing and molding: The composite material obtained in step (3) is placed in an oven for baking and curing to obtain a highly oriented boron nitride composite material.

[0011] Furthermore, in step (1), 100 ml of surfactant solution with a concentration of 0.2 mol / L, 50 ml of hydrochloric acid solution with a concentration of 0.1 mol / L, and 0.5 g to 0.75 g of hexagonal boron nitride are used to adjust the pH value of the solution to less than 4.

[0012] Furthermore, in step (2), 100 ml of FeCl3 solution with a concentration of 0.2 mol / L, 100 ml of FeCl2 solution with a concentration of 0.1 mol / L, 50 ml of sodium hydroxide with a concentration of 0.1 mol / L, and 25 ml of 25% ammonia solution are added to the mixed solution of step (1).

[0013] Furthermore, in the step (3), the resin matrix is ​​100 ml, the magnetic induction intensity is controlled to be 0.1-0.3 T, initially 0.1 T, and the magnetic induction intensity is continued to increase after the magnetic treatment, and the increase rate is controlled to be 0.1 T / h.

[0014] Furthermore, in step (4), the oven temperature is controlled at 80° C.-90° C., and the curing time is 30 min-40 min.

[0015] Furthermore, the surfactant solution includes one or more of sodium polystyrene sulfonate, sodium dodecyl sulfate, and ammonium dodecyl sulfate.

[0016] Furthermore, the resin matrix includes one or more of polyetherimide, epoxy resin, polyimide, and phenolic resin.

[0017] Compared with the prior art, the present invention has the following advantages:

[0018] The present invention adopts magnetic treatment to obtain a deposited magnetic enhancement layer, and uses a surfactant to perform surface treatment on hexagonal boron nitride, so that it can be used as a bridge between the magnetic material and the hexagonal boron nitride particles, thereby giving the hexagonal boron nitride magnetic activity, making it possible for the boron nitride to be arranged along the target direction, and at the same time, parameters such as temperature, magnetic induction intensity, and magnetic treatment time can be adjusted to obtain boron nitride composite materials with different magnetic activities, deposition quality, and magnetic deflection angles. At the same time, performance tests have proved that the core-shell structure can improve the dispersion and orientation of fillers, can significantly improve the heat dissipation capacity of electronic components, can effectively improve the insulation performance of composite materials, and has great application potential in thermal conductive composite materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 This is a flow chart for the preparation of hexagonal boron nitride thermal conductive composite materials. DETAILED DESCRIPTION

[0020] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be further described below.

[0021] Embodiment 1:

[0022] The preparation method of the hexagonal boron nitride composite material of this embodiment comprises the following steps:

[0023] Step (1): Sodium polystyrene sulfonate is used as a surfactant for hexagonal boron nitride, which is a bridge between magnetic ferrite and hexagonal boron nitride particles. During the activation process, the concentration of the solution can be adjusted to a certain extent. 100 ml of sodium polystyrene sulfonate, the solution concentration is 0.2 mol / L, add 50 ml of hydrochloric acid solution, the concentration is 0.1 mol / L, add 0.5 g h-BN (hexagonal boron nitride), and then add 1 mol / L of HCL to adjust the pH value of the solution to less than 4.

[0024] Step (2): Add 100 ml of FeCl3 solution with a concentration of 0.2 mol / L to the mixed solution of step (1). Add 100 ml of FeCl2 solution with a concentration of 0.1 mol / L to achieve Fe 3+ with Fe 2+ The molar ratio of sodium hydroxide is controlled at 2:1, and 50 ml of sodium hydroxide is added to a solution concentration of 0.1 mol / L. 25 ml of 25% ammonia solution is added. Sodium hydroxide and ammonia water are combined with iron ions to obtain Fe3O4 nanoparticles through coprecipitation. Sodium polystyrene sulfonate is an ionic polymer that introduces negative charges on the surface of hexagonal boron nitride to attract Fe 3+ and Fe 2+Attached to the surface of hexagonal boron nitride. Then add 1,6-hexanediamine solution to the mixture, the concentration is controlled to be 0.5 mol / L, as the base of the mixed solution, take deionized water, filter and wash with deionized water three times to remove excess amine molecules, control the temperature to 90°C and dry into powder to obtain hexagonal boron nitride material with magnetic activity.

[0025] Step (3): Magnetic treatment: Add 100 ml of 0.5 mol / L polyetherimide to the material obtained in step (2) as the matrix of the composite material, and perform magnetic treatment. The magnetic induction intensity is controlled to be 0.1-0.3 T, initially 0.1 T. After the magnetic treatment, the magnetic induction intensity is continuously increased, and the increase rate is controlled to be 0.1 T / h. The purpose of increasing the magnetic field intensity is to enable the hexagonal boron nitride thermal conductive particles to form a complete oriented structure. The direction of the magnetic field is controlled to be vertical, and the magnetic treatment time is 2 hours, in order to obtain a hexagonal boron nitride composite material with high thermal conductivity in a highly arranged vertical direction.

[0026] Step (4): Heat and cure the mold: The composite material obtained in step (3) is placed in an oven for baking and curing. The oven temperature is controlled at 90°C and the curing time is generally 30 minutes to obtain a highly oriented boron nitride composite material.

[0027] After magnetized iron oxide deposition, the magnetic iron oxide is evenly wrapped on the hexagonal boron nitride to form a core-shell structure, which greatly broadens the heat conduction path and increases the contact probability between fillers.

[0028] Comparative Example 1:

[0029] The method for preparing the hexagonal boron nitride composite material of this comparative example is different from that of Example 1 in that the thermally conductive hexagonal boron nitride composite material is not subjected to a magnetic treatment process.

[0030] The properties of the hexagonal boron nitride / polyetherimide composite material, the unmagnetized hexagonal boron nitride / polyetherimide composite material, and the pure polyetherimide resin material prepared by the preparation methods of Example 1 and Comparative Example 1 are as follows:

[0031] The out-of-plane thermal conductivity of the hexagonal boron nitride / polyetherimide composite material after magnetic treatment for 2h can reach 1.67W / mK. At this time, the magnetic iron oxide content can reach 7wt%. Compared with the unmagnetized hexagonal boron nitride / polyetherimide composite material and pure polyetherimide resin material, the thermal conductivity of the boron nitride composite material after high temperature treatment has been greatly improved. The boron nitride composite material after magnetic treatment also shows certain negative dielectric properties and dielectric loss is also small. Its in-plane AC conductivity is 0.02S / cm at 10kHz, and the dielectric loss is only 1.10.

[0032] The preparation method of pure polyetherimide resin material is as follows: the pure polyetherimide resin material is prepared by heating 4,4'-diaminodiphenyl ether or m-(or p-)phenylenediamine and 2,2'-bis[4-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride in dimethylacetamide solvent for polycondensation, powdering and imidization.

[0033] Comparative Example 2:

[0034] The method for preparing the hexagonal boron nitride composite material in this example is different from that in Example 1 in that the boron nitride content is increased to 30 wt % (0.75 g h-BN (hexagonal boron nitride) is added).

[0035] Comparative Example 3:

[0036] The hexagonal boron nitride composite material and preparation method thereof in this example are different from those in Example 1 in that the magnetic treatment time of the thermally conductive hexagonal boron nitride composite material is 0.5 h.

[0037] The properties of the hexagonal boron nitride / polyetherimide composite material and the pure polyetherimide resin material prepared by the preparation methods of Comparative Examples 2 and 3 are as follows:

[0038] The in-plane thermal conductivity of the hexagonal boron nitride / polyetherimide composite material after magnetic treatment for 0.5h is 1.10 W / mK, which is significantly reduced compared with the hexagonal boron nitride / polyetherimide composite material and pure polyetherimide resin material after magnetic treatment for 2h. It can be seen that the magnetic treatment time has a great influence on the arrangement of fillers. Its in-plane AC conductivity is 0.06S / cm at 10kHz, and the dielectric loss is only 1.10.

[0039] The properties of the hexagonal boron nitride / polyetherimide composite material and the pure polyetherimide resin material prepared by the preparation methods of Comparative Examples 2 and 3 are as follows:

[0040] The in-plane W / mK of the hexagonal boron nitride / polyetherimide composite material after magnetic treatment for 2 hours has a relatively large filler content (20wt%). Compared with the hexagonal boron nitride / polyetherimide composite material with a filler content of 20wt% and the pure polyetherimide resin material, the thermal conductivity of the boron nitride composite material with a filler content of 30wt% has been greatly improved, and the increased filler content will not have a significant impact on the mechanical properties of the composite material.

[0041] Its in-plane AC conductivity is 0.04S / cm at 10kHz and its dielectric loss is only 1.03.

[0042]

[0043] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any technician in the relevant technical field, without departing from the scope of the technical solution of the present invention, makes any form of equivalent replacement or modification to the technical solution and technical content disclosed in the present invention, which does not depart from the content of the technical solution of the present invention and still falls within the protection scope of the present invention.

Claims

1. A hexagonal boron nitride composite material, characterized in that: The invention comprises a resin matrix and core-shell particles which are distributed in the matrix in a direction. The core of the core-shell particles is hexagonal boron nitride modified by a surfactant, and the shell layer is a magnetic material.

2. A thermally conductive composite material, characterized in that: It is made from the hexagonal boron nitride composite material described in claim 1.

3. The method for preparing the hexagonal boron nitride composite material according to claim 1, characterized in that: The steps include: (1) adding a hydrochloric acid solution to a surfactant solution, and then adding hexagonal boron nitride to adjust the pH value of the solution; (2) Add FeCl3 solution and FeCl2 solution to the mixed solution of step (1) to achieve Fe 3+ with Fe 2+ The molar ratio of is controlled at 2:1, sodium hydroxide solution and ammonia solution are added, and then 1,6-hexanediamine solution is added to the mixture, and the mixture is filtered and washed three times with deionized water to remove excess amine molecules, and dried to obtain a hexagonal boron nitride material with magnetic activity; (3) Magnetic treatment: adding a resin matrix to the material obtained in step (2) to perform magnetic treatment, and after the magnetic treatment, continuing to increase the magnetic induction intensity, and controlling the direction of the magnetic field to be in the vertical direction; (4) Curing and molding: The composite material obtained in step (3) is placed in an oven for baking and curing to obtain a highly oriented boron nitride composite material.

4. The method for preparing the hexagonal boron nitride composite material according to claim 3, characterized in that: In the step (1), 100 ml of surfactant solution with a concentration of 0.2 mol / L, 50 ml of hydrochloric acid solution with a concentration of 0.1 mol / L, and 0.5 g to 0.75 g of hexagonal boron nitride are used to adjust the pH value of the solution to less than 4.

5. The method for preparing the hexagonal boron nitride composite material according to claim 3, characterized in that: In the step (2), 100 ml of FeCl3 solution with a concentration of 0.2 mol / L, 100 ml of FeCl2 solution with a concentration of 0.1 mol / L, 50 ml of sodium hydroxide with a concentration of 0.1 mol / L, and 25 ml of 25% ammonia solution are added to the mixed solution of step (1).

6. The method for preparing the hexagonal boron nitride composite material according to claim 3, characterized in that: In the step (3), the magnetic induction intensity of the resin matrix is ​​100 ml and is controlled to be 0.1-0.3 T, initially 0.1 T. After the magnetic treatment is completed, the magnetic induction intensity is continuously increased and the increasing rate is controlled to be 0.1 T / h.

7. The method for preparing the hexagonal boron nitride composite material according to claim 3, characterized in that: In the step (4), the oven temperature is controlled at 80° C.-90° C., and the curing time is 30 min-40 min.

8. The method for preparing the hexagonal boron nitride composite material according to claim 3, characterized in that: The surfactant solution includes one or more of sodium polystyrene sulfonate, sodium dodecyl sulfate, and ammonium dodecyl sulfate.

9. The method for preparing the hexagonal boron nitride composite material according to claim 3, characterized in that: The resin matrix includes one or more of polyetherimide, epoxy resin, polyimide, and phenolic resin.

Citation Information

Cited By

  • Hexagonal boron nitride / sphere-like filler heat-conducting butadiene-styrene copolymer composite material as well as preparation method and application thereof

    CN120310087A