Polishing composition for polishing organic dielectric layer and manufacturing method of semiconductor device
By using abrasive solution and surfactant in the polishing composition in the polishing composition, the problem of grinding defects during chemical mechanical polishing is solved, and the planarization effect of organic dielectric layer and semiconductor devices are improved. The yield rate achieves efficient polishing rate and selection ratio.
Patent Information
- Application Number
- CN202411088123.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-22
AI Technical Summary
During the chemical mechanical polishing process, traditional abrasive slurry is prone to cause abrasive defects, affecting the planarization effect of the organic spin-coated dielectric layer, and has poor yield and polishing rate of semiconductor devices.
Provided is a polishing composition for polishing an organic dielectric layer, including components A and components B, components A are abrasive solutions, and components B include surfactant and additive 4-hydroxybenzoic acid to improve polishing by synergistic action Grinding defects during the process and adjust the ratio to increase the polishing rate and selection ratio.
It effectively improves the abrasive defects during the polishing process, improves the planarization effect of the organic dielectric layer and the yield of semiconductor devices, improves the polishing rate and selection ratio, and ensures the stability of the polishing effect.
Smart Images

Figure CN118995053A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of polishing liquid, and in particular to a polishing composition for polishing an organic medium layer and a method for manufacturing a semiconductor device. Background Art
[0002] At present, the development trend of memory chips is that the feature size is getting smaller and smaller, and the number of stacked layers is getting larger and larger, which has higher requirements for filling technology and chemical mechanical polishing (CMP) planarization technology. For example, in the phase change memory (PCM) memory process, the filling technology of organic spin-on dielectric (SOD) has begun to be used to fill high aspect ratio memory cells. However, when performing chemical mechanical polishing on organic spin-on dielectrics, traditional polishing slurries are prone to cause polishing defects. Summary of the invention
[0003] The present application provides a polishing composition for polishing an organic dielectric layer and a method for manufacturing a semiconductor device, which improves grinding defects during the polishing process to at least solve some of the above problems.
[0004] In a first aspect, the present application provides a polishing composition for polishing an organic medium layer, comprising a component A and a component B, wherein the component A is an abrasive solution, and the component B comprises a surfactant and an additive, wherein the additive is 4-hydroxybenzoic acid.
[0005] In some embodiments, the B component includes the following components, calculated by weight percentage:
[0006]
[0007] In some embodiments, in the B component, the mass ratio of the surfactant to the additive is (0.6-1.5):1.
[0008] In some embodiments, the first pH regulator is selected from at least one of an organic acid and an organic base; and / or,
[0009] The surfactant is selected from at least one of fatty alcohol polyoxyethylene ether, fatty acid polyoxyethylene ester and alkylphenol polyoxyethylene ether; and / or,
[0010] The B component is an acidic solution.
[0011] In some embodiments, the A component includes the following components, calculated by weight percentage:
[0012]
[0013] In some embodiments, the abrasive is a cerium dioxide sol, and the solid content of the cerium dioxide sol is 5% to 40%; and / or, the particle size of the cerium dioxide sol is 150nm to 350nm; and / or,
[0014] The dispersant is methyl amyl alcohol; and / or,
[0015] The chelating agent is at least one selected from FA / O chelating agent, tetrahydroxyethylethylenediamine, ethylenediamine and triethanolamine; and / or,
[0016] The second pH regulator is selected from at least one of an organic acid and an organic base; and / or,
[0017] The A component is an acidic solution.
[0018] In some embodiments, the polishing composition comprises:
[0019] Component A: 20 wt% to 50 wt%;
[0020] Component B 8wt% to 15wt%; and
[0021] Water, balance.
[0022] In some embodiments, the polishing composition is an acidic solution.
[0023] In some embodiments, the organic medium layer includes a C element.
[0024] In a second aspect, the present application provides a method for manufacturing a semiconductor device, comprising the following steps:
[0025] Providing the above-mentioned component A and the above-mentioned component B, and mixing the two to obtain a polishing composition for polishing an organic medium layer;
[0026] Providing a semiconductor structure, the semiconductor structure comprising an organic dielectric layer and an inorganic layer, the organic dielectric layer covering the inorganic layer; and
[0027] A polishing pad and the polishing composition are used to remove a portion of the organic medium layer until the inorganic layer is exposed, thereby obtaining a polished organic medium layer.
[0028] In the polishing composition for polishing the organic medium layer of some embodiments provided in the present application, component A is an abrasive solution. Component B includes additives 4-hydroxybenzoic acid and a surfactant, and 4-hydroxybenzoic acid and the surfactant work together to improve the grinding defects during the polishing process. Component A and component B are matched with each other in a certain ratio to improve the grinding defects during the polishing process and improve the polishing rate and selectivity of the polishing composition during the polishing process. In addition, by adjusting the ratio of component A and component B, the polishing performance of the polishing composition during the polishing process can be adjusted more flexibly. Furthermore, compared with directly adding additives and surfactants to component A, separating component B from component A can better ensure that the additives and surfactants in component B are more evenly dispersed when mixed with component A, and then play a corresponding role in the polishing process, improving the problem that components such as additives and surfactants are directly attached to the abrasive and are difficult to play a role and affect the polishing effect.
[0029] In the semiconductor device manufacturing method of some embodiments of the present application, the above-mentioned polishing composition is used to planarize the organic dielectric layer of the semiconductor structure, which not only improves the planarization effect of the organic dielectric layer and improves the over-grinding defects in the polishing process, but also improves the yield of the semiconductor device. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1A to Figure 1B A schematic diagram of a process for manufacturing semiconductor devices according to some embodiments of the present application;
[0031] Figure 2 and Figure 3 The figures are after the wafers are treated with the polishing compositions or polishing liquids of Example 1 and the comparative example. DETAILED DESCRIPTION
[0032] The technical solutions in the embodiments of the present application will be described clearly and completely below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present application.
[0033] In a first aspect, the present application provides a polishing composition for polishing an organic medium layer. The polishing composition comprises a component A and a component B, that is, the polishing composition comprises two components. Before use, the component A and the component B are mixed evenly to obtain a polishing composition. The component A is an abrasive solution. The component B comprises a surfactant and an additive. The additive is 4-hydroxybenzoic acid.
[0034] In the polishing composition for polishing the organic medium layer in some embodiments of the present application, component A is an abrasive solution. Component B includes additives 4-hydroxybenzoic acid and a surfactant, and 4-hydroxybenzoic acid and the surfactant work together to improve the grinding defects during the polishing process. Component A and component B are matched with each other in a certain ratio to improve the grinding defects during the polishing process and improve the polishing rate and selectivity of the polishing composition during the polishing process. In addition, by adjusting the ratio of component A and component B, the polishing performance of the polishing composition during the polishing process can be adjusted more flexibly. Furthermore, compared with directly adding additives and surfactants to component A, separating component B from component A can better ensure that the additives and surfactants in component B are more evenly dispersed when mixed with component A, and then play a corresponding role in the polishing process, improving the problem that components such as additives and surfactants are directly attached to the abrasive and are difficult to play a role and affect the polishing effect.
[0035] In some embodiments, the thickness of the organic dielectric layer is 1000 angstroms to 3000 angstroms, so as to ensure the filling effect when the organic dielectric layer is used as a filling material. Optionally, the thickness of the organic dielectric layer is 1500 angstroms to 2500 angstroms.
[0036] In some embodiments, the hardness of the organic medium layer is 1.3 GPa to 1.5 GPa, so that the hardness of the organic medium layer is relatively large.
[0037] In some embodiments, the modulus of the organic dielectric layer is 10 GPa to 12 GPa, so as to ensure that the modulus of the organic dielectric layer is relatively large.
[0038] The organic medium layer includes C element to ensure that the organic medium layer has a certain hardness. In some embodiments, the number of atoms of C element in the organic medium layer accounts for 12% to 15%.
[0039] In some embodiments, the organic dielectric layer further includes Si element and O element, the atomic number of O element in the organic dielectric layer accounts for 45% to 58%, and the atomic number of Si element in the organic dielectric layer accounts for 30% to 41%.
[0040] In some embodiments, the organic dielectric layer includes Si-O bonds and Si-R bonds, and the R alkyl group may include an alkyl group of 1 to 20 carbon elements. Alternatively, the R alkyl group may include an alkyl group of 1 to 10 carbon elements. Alternatively, the R alkyl group may include an alkyl group of 1 to 8 carbon elements. Alternatively, the R alkyl group may include an alkyl group of 1 to 4 carbon elements.
[0041] Exemplarily, a partial structure of the material of the organic dielectric layer is as follows:
[0042]
[0043] In some embodiments, the organic dielectric layer can be prepared by filling the gap with an initial organic material through a spin coating process, and then performing a baking and curing process on the initial organic material.
[0044] In some embodiments, component A includes the following components, calculated by mass percentage: 0.05 wt% to 4 wt% abrasive, 0.05 wt% to 0.5 wt% dispersant, 0 wt% to 1 wt% chelating agent, 0 wt% to 0.5 wt% second pH adjuster, and the balance water.
[0045] In some embodiments, component A comprises the following components, calculated by mass percentage: 1.2 wt% to 3.8 wt% abrasive, 0.1 wt% to 0.4 wt% dispersant; 0.01 wt% to 1 wt% chelating agent, 0 wt% to 0.5 wt% second pH regulator and the balance water.
[0046] In some embodiments, in component A, the mass percentage of the abrasive can also be 0.08wt% to 3.8wt%, 0.15wt% to 3.6wt%, 0.3wt% to 3.4wt%, 0.8wt% to 3.2wt%, 1.2wt% to 3.0wt%, 1.5wt% to 2.8wt% or 1.8wt% to 2.5wt%.
[0047] It is understood that, in component A, the mass percentage of abrasive can be selected from any value between 0.05wt% and 4wt%. Exemplarily, the mass percentage of abrasive is 0.05wt%, 0.1wt%, 0.15wt%, 0.25wt%, 0.35wt%, 0.45wt%, 0.75wt%, 1wt%, 1.2wt%, 1.5wt%, 1.8wt%, 2.0wt%, 2.2wt%, 2.5wt%, 2.8wt%, 3.2wt%, 3.4wt%, 3.6wt%, 3.8wt% or 4.0wt%, but is not limited thereto.
[0048] In some embodiments, the abrasive is a cerium dioxide sol. The cerium dioxide sol has a high removal rate for the organic medium layer including the C element, thereby ensuring a high polishing rate of the polishing composition for the organic medium layer including the C element. In addition, the cerium dioxide sol can overcome the shortcomings of uneven particle size distribution, high hardness, and easy coagulation of solid-phase cerium dioxide abrasives, thereby improving the polishing efficiency of the polishing composition. The cerium dioxide sol can be synthesized by a common chemical method, which will not be described in detail here.
[0049] In some embodiments, the solid content of the ceria sol is 5% to 40%. Thus, the ceria sol has a suitable solid content to ensure that the polishing composition has a high polishing rate for the organic medium layer while reducing the risk of gelation of the ceria sol.
[0050] In some embodiments, the solid content of the ceria sol may be 8% to 35%, 12% to 30%, 15% to 25%, or 18% to 22%.
[0051] It is understood that the solid content of the ceria sol can be selected from any value between 5% and 40%. For example, the solid content of the ceria sol can be 5%, 8%, 12%, 16%, 20%, 24%, 28%, 32%, 36% or 40%.
[0052] In some embodiments, the particle size of the ceria sol is 150 nm to 350 nm. Thus, the ceria sol has a suitable particle size to reduce the risk of ceria sol aggregation and deposition, while ensuring that the polishing composition has a high polishing rate for the organic medium layer, and reduces the risk of causing polishing surface defects, thereby improving the polishing effect.
[0053] In some embodiments, the particle size of the ceria sol may also be 155 nm to 320 nm, 160 nm to 280 nm, 165 nm to 270 nm, or 170 nm to 250 nm.
[0054] It is understood that the particle size of the ceria sol can be selected from any value between 150nm and 350nm. For example, the particle size of the ceria sol can be 150nm, 170nm, 180nm, 190nm, 210nm, 230nm, 250nm, 270nm, 300nm or 320nm.
[0055] The dispersant plays a role in dispersing the abrasive, reducing the risk of abrasive aggregation and deposition, so as to improve the stability of the abrasive in component A. In some embodiments, the dispersant is methylpentanol, so as to improve the stability of the ceria sol in component A.
[0056] In some embodiments, in component A, the mass percentage of the dispersant may be 0.08 wt% to 0.45 wt%, 0.1 wt% to 0.4 wt%, 0.15 wt% to 0.35 wt%, or 0.2 wt% to 0.28 wt%.
[0057] It is understood that in component A, the mass percentage of the dispersant can be selected from any value between 0.05wt% and 0.5wt%. Exemplarily, the mass percentage of the dispersant is 0.05wt%, 0.1wt%, 0.15wt%, 0.2wt%, 0.25wt%, 0.3wt%, 0.35wt%, 0.4wt%, 0.45wt% or 0.5wt%.
[0058] The chelating agent plays a role in chelating the metal ions in the polishing process, reducing the problem that the polishing residue generated by polishing condenses on the polishing surface of the organic medium layer and affects the polishing efficiency. In some embodiments, the chelating agent is selected from at least one of FA / O chelating agent, tetrahydroxyethylethylenediamine, ethylenediamine and triethanolamine. Optionally, the chelating agent is tetrahydroxyethylethylenediamine.
[0059] In some embodiments, in component A, the mass percentage of the chelating agent may be 0.01 wt% to 0.8 wt%, 0.05 wt% to 0.7 wt%, 0.1 wt% to 0.6 wt%, 0.2 wt% to 0.5 wt%, or 0.25 wt% to 0.4 wt%.
[0060] It is understood that in component A, the mass percentage of the chelating agent can be selected from any value between 0wt% and 1wt%. Exemplarily, the mass percentage of the dispersant is 0.05wt%, 0.1wt%, 0.15wt%, 0.2wt%, 0.25wt%, 0.3wt%, 0.35wt%, 0.4wt%, 0.45wt%, 0.5wt%, 0.55wt%, 0.6wt%, 0.65wt%, 0.7wt%, 0.75wt%, 0.8wt%, 0.85wt%, 0.9wt% or 0.95wt%.
[0061] In some embodiments, component B includes the following components, calculated by mass percentage: 0 wt% to 0.5 wt% of a first pH adjuster, 0.01 wt% to 0.5 wt% of a surfactant, 0.01 wt% to 1 wt% of an additive, and the balance of water.
[0062] In some embodiments, component B comprises the following components, calculated by weight percentage: 0 wt% to 0.5 wt% of a first pH adjuster, 0.05 wt% to 0.5 wt% of a surfactant, 0.1 wt% to 0.5 wt% of an additive, and the balance of water.
[0063] In the process of chemical mechanical polishing, surfactants can play multiple roles such as corrosion protection and abrasive dispersion. When the polishing surface is uneven, the corrosion protection can reduce the polishing rate of the abrasive at the concave position, protect the structure at the concave position, reduce the risk of over-grinding, and improve the flattening effect. The abrasive dispersion can reduce the risk of abrasive aggregation.
[0064] In some embodiments, in component B, the mass percentage of the surfactant may be 0.03 wt% to 0.45 wt%, 0.05 wt% to 0.4 wt%, 0.1 wt% to 0.35 wt%, or 0.25 wt% to 0.45 wt%.
[0065] It is understood that in component B, the mass percentage of the surfactant can be any value between 0.01wt% and 0.5wt%. For example, the mass percentage of the surfactant can be 0.01wt%, 0.03wt%, 0.05wt%, 0.1wt%, 0.15wt%, 0.2wt%, 0.25wt%, 0.3wt%, 0.35wt%, 0.4wt%, 0.45wt% or 0.5wt%.
[0066] In certain embodiments, the surfactant is a nonionic surfactant. The nonionic surfactant is selected from at least one of fatty alcohol polyoxyethylene ether, fatty acid polyoxyethylene ester and alkylphenol polyoxyethylene ether. In this way, the nonionic surfactant plays a good role in corrosion protection and abrasive dispersion. Optionally, the nonionic surfactant is fatty alcohol polyoxyethylene ether.
[0067] As an additive, 4-hydroxybenzoic acid has almost no effect on the removal rate of the organic dielectric layer, and can also effectively reduce the removal rate of other materials outside the organic dielectric layer, and improve the selectivity of the polishing composition. The synergy between 4-hydroxybenzoic acid and the surfactant can not only improve the grinding defects caused by over-grinding, but also improve the selectivity of the organic dielectric layer and other materials.
[0068] In some embodiments, in component B, the mass percentage of the additive may be 0.05 wt% to 0.8 wt%, 0.08 wt% to 0.7 wt%, 0.1 wt% to 0.6 wt%, 0.15 wt% to 0.5 wt%, 0.2 wt% to 0.5 wt%, or 0.25 wt% to 0.45 wt%.
[0069] In some embodiments, in component B, the mass percentage of the additive may be any value between 0.01 wt% and 1 wt%. For example, the mass percentage of the additive may be 0.01 wt%, 0.03 wt%, 0.05 wt%, 0.1 wt%, 0.15 wt%, 0.2 wt%, 0.25 wt%, 0.3 wt%, 0.35 wt%, 0.4 wt%, 0.45 wt%, 0.5 wt%, 0.6 wt%, 0.7 wt%, 0.8 wt% or 0.9 wt%.
[0070] In some embodiments, in component B, the mass ratio of the surfactant to the additive is (0.6-1.5): 1. In this way, the grinding defects in the grinding process can be better improved, and the polishing composition can be ensured to have a high selectivity ratio for the organic medium layer and other materials.
[0071] In some embodiments, in component B, the mass ratio of the surfactant to the additive may be (0.8-1.2): 1. In this way, the grinding defects during the grinding process can be further improved, and the polishing composition can be further guaranteed to have a high selectivity ratio for the organic dielectric layer and other materials.
[0072] It is understood that in component B, the mass ratio of the surfactant to the additive may be any value between (0.6-1.5): 1. For example, the mass ratio of the surfactant to the additive may be 0.6:1, 0.7:1, 0.8:1, 0.9:1, 1:1, 1.2:1, 1.4:1 or 1.5:1.
[0073] In some embodiments, in component A and component B, the first pH regulator and the second pH regulator are each independently selected from at least one of an organic acid and an organic base. In this way, the pH value of component A and component B can be adjusted. The organic acid may include but is not limited to citric acid. The organic base may include but is not limited to tetraethylammonium hydroxide.
[0074] In some embodiments, component A is an acidic solution. In this way, the risk of abrasive aggregation is reduced when the abrasive is a ceria sol. In some embodiments, the pH value of component A can be 4.2 to 6. Exemplarily, the pH value of component A can be 4.2, 4.4, 4.6, 4.8, 5.0, 5.2, 5.4, 5.6, 5.8 or 6.0.
[0075] In some embodiments, component B is an acidic solution. Thus, when component B is mixed with component A, the risk of abrasive aggregation is reduced when the abrasive is a ceria sol. In some embodiments, the pH value of component B may be 4.2 to 6. Exemplarily, the pH value of component B may be 4.2, 4.4, 4.6, 4.8, 5.0, 5.2, 5.4, 5.6, 5.8 or 6.0.
[0076] In some embodiments, the water is deionized water.
[0077] In some embodiments, the polishing composition includes, by weight percentage, 20 wt% to 50 wt% of component A; 8 wt% to 15 wt% of component B; and the balance of water. Thus, component A and component B have a suitable ratio, ensuring that the polishing composition formed after the two are mixed has a high polishing rate and a high selectivity for the organic dielectric layer, improving the over-polishing problem during the polishing process of the organic dielectric layer, and obtaining a better planarization effect.
[0078] In some embodiments, the polishing composition includes, calculated by mass percentage: 25 wt% to 45 wt% of component A; 10 wt% to 14 wt% of component B; and the balance of water.
[0079] In some embodiments, in the polishing composition, the mass percentage of component A can be any value between 20 wt % and 50 wt %. For example, in the polishing composition, the mass percentage of component A can be 20 wt %, 25 wt %, 30 wt %, 35 wt %, 40 wt %, 45 wt % or 50 wt %.
[0080] In some embodiments, in the polishing composition, the mass percentage of component B can be any value between 8 wt% and 15 wt%. For example, in the polishing composition, the mass percentage of component B can be 8 wt%, 8.5 wt%, 9 wt%, 9.5 wt%, 10 wt%, 10.5 wt%, 11 wt%, 11.5 wt%, 12 wt%, 12.5 wt%, 13 wt%, 13.5 wt%, 14 wt% or 15 wt%.
[0081] In some embodiments, the polishing composition is an acidic solution, and the pH value of the polishing composition is 4.2 to 6. In this way, the polishing composition is guaranteed to have a suitable polishing rate. Optionally, the pH value of the polishing composition is 4.5 to 5.8.
[0082] It is understood that the pH value of the polishing composition can be any value between 4.2 and 6. For example, the pH value of the polishing composition can be 4.2, 4.4, 4.6, 4.8, 5.0, 5.2, 5.4, 5.6, 5.8 or 6.0.
[0083] The polishing composition for polishing the organic dielectric layer can effectively improve the grinding defects in the polishing process, and improve the removal rate, selectivity and polishing rate of the organic dielectric layer, and the polishing effect has good stability.
[0084] In a second aspect, the present application also provides a method for manufacturing a semiconductor device, comprising the following steps:
[0085] Step S101: providing the above-mentioned component A and the above-mentioned component B, and mixing the two to obtain a polishing composition for polishing an organic medium layer;
[0086] Step S102: providing a semiconductor structure, the semiconductor structure comprising an organic dielectric layer and an inorganic layer, the organic dielectric layer covering the inorganic layer; and
[0087] Step S103: using a polishing pad and the polishing composition to remove a portion of the organic dielectric layer until the inorganic layer is exposed, thereby obtaining a polished organic dielectric layer.
[0088] In some embodiments, the semiconductor device may be a memory, a wafer, or other semiconductor devices.
[0089] In some embodiments, in step S101, mixing the two includes: mixing the above component A with the above component B, and stirring them evenly.
[0090] In some embodiments, in step S102, Figure 1A As shown, the semiconductor structure 100 may include a storage stack 11, which may be disposed on the substrate 10 or inside the substrate 10. The storage stack 11 includes a gap 11A between a plurality of storage cells, and an organic dielectric layer 13 is filled in the gap 11A to perform filling and insulation functions. The gap 11A may be a gap with a high aspect ratio. Figure 1A and Figure 1B As shown, the inorganic layer 12 is disposed on the storage stack 11 , and the organic medium layer 13 covers the inorganic layer 12 .
[0091] In some embodiments, the storage stack 11 may include a storage layer, which may be at least one of a phase change storage layer and a bidirectional threshold switching layer. The storage stack 11 may also include a word line layer and a bit line layer, wherein the storage layer is disposed between the word line layer and the bit line layer. The storage stack 11 may also include an electrode layer stacked with the storage layer.
[0092] like Figure 1B As shown, in step S103 , the planarization process of the organic dielectric layer 13 stops on the inorganic layer 12 .
[0093] In some embodiments, the inorganic layer 12 may include at least one of silicon nitride, silicon oxide, and silicon oxynitride. Exemplarily, the inorganic layer 12 includes silicon nitride.
[0094] It should be noted that, when the inorganic layer is a silicon nitride layer, the composition of the polishing composition is selected so that the polishing rate of the silicon nitride layer by the polishing composition is low. Therefore, the polishing composition has a high selectivity ratio between the organic dielectric layer 13 and the silicon nitride layer, reduces the risk of over-polishing the silicon nitride layer, improves the planarization effect of the organic dielectric layer 13, and also improves the problem of defects caused by over-grinding of the silicon nitride layer during the polishing process.
[0095] The performance of the polishing composition is verified in combination with specific examples and comparative examples. The SOD material in the following is purchased from Merck SOD RS2000. The materials in other examples and comparative examples are also commercially available and will not be described in detail here.
[0096] Example 1
[0097] This embodiment provides a method for preparing a polishing composition, comprising the following steps:
[0098] Preparation of component A:Take an abrasive (40 g of cerium dioxide sol with a mass fraction of 40% and a particle size of 150 nm to 350 nm), 10 g of a chelating agent (tetrahydroxyethylethylenediamine), 2 g of a dispersant (methylpentanol) and a pH regulator (citric acid and tetraethylammonium hydroxide); then, add the abrasive, chelating agent and dispersant to an appropriate amount of deionized water in sequence, stir evenly by step-by-step mixing, fill with deionized water to make component A 1000 g, and continue stirring evenly; finally, use a pH regulator to adjust the pH value to 5 to obtain component A.
[0099] Preparation of component B: Take 5 g of non-ionic surfactant (fatty alcohol polyoxyethylene ether AEO7) and 5 g of additive (4-hydroxybenzoic acid); then, add the non-ionic surfactant and additive components to an appropriate amount of deionized water in turn, stir evenly by step-by-step mixing, make up to 1000 g of component B with deionized water, and continue to stir evenly; finally, use a pH regulator to adjust the pH value to 5 to obtain component B.
[0100] Mix components A and B: Take 3 parts of the above component A, 1.25 parts of the component B and 5.75 parts of deionized water, mix them evenly, and obtain the polishing composition of this embodiment.
[0101] Example 2
[0102] This embodiment provides a method for preparing a polishing composition. This embodiment is basically similar to Embodiment 1, and the steps for preparing component A and component B are the same, except for the step of mixing component A and component B. In this embodiment, the step of mixing component A and component B is to take 5 parts of component A, 0.8 parts of component B and 4.2 parts of deionized water, and mix them evenly to obtain the polishing composition of this embodiment.
[0103] Example 3
[0104] This embodiment provides a method for preparing a polishing composition. This embodiment is basically similar to Embodiment 1, and the steps for preparing component A and component B are the same, except for the step of mixing component A and component B. In this embodiment, the step of mixing component A and component B is to take 2 parts of component A, 1.5 parts of component B and 6.5 parts of deionized water, mix them evenly, and obtain the polishing composition of this embodiment.
[0105] Example 4
[0106] This embodiment provides a method for preparing a polishing composition. This embodiment is basically similar to Embodiment 1, except for the step of preparing component B, and the other steps are the same. In this embodiment, the step of preparing component B is: taking 3g of nonionic surfactant (fatty alcohol polyoxyethylene ether AEO7) and 5g of additive (4-hydroxybenzoic acid); then, adding the nonionic surfactant and the additive components to an appropriate amount of deionized water in sequence, stirring evenly by step-by-step mixing, and filling up with deionized water until component B is 1000g, and continuing to stir evenly; finally, using a pH regulator to adjust the pH value to 5 to obtain component B.
[0107] Example 5
[0108] This embodiment provides a method for preparing a polishing composition. This embodiment is basically similar to Embodiment 1, except for the step of preparing component B, and the other steps are the same. In this embodiment, the step of preparing component B is: taking 4.5g of nonionic surfactant (fatty alcohol polyoxyethylene ether AEO7) and 3g of additive (4-hydroxybenzoic acid); then, adding the nonionic surfactant and the additive components to an appropriate amount of deionized water in sequence, stirring evenly by step-by-step mixing, and filling up with deionized water until component B is 1000g, and continuing to stir evenly; finally, using a pH regulator to adjust the pH value to 5 to obtain component B.
[0109] Comparative Example 1
[0110] The cerium dioxide polishing liquid STI2503 produced by Merck in Germany and purchased on the market.
[0111] Comparative Example 2
[0112] The cerium dioxide polishing liquid D2021 produced by Anjie Technology purchased on the market.
[0113] Comparative Example 3
[0114] The cerium dioxide polishing liquid HS0231 produced by Hitachi of Japan and purchased on the market.
[0115] Comparative Example 4
[0116] This comparative example is basically similar to Example 1, except that no nonionic surfactant is added when preparing component B.
[0117] Comparative Example 5
[0118] This comparative example is substantially similar to Example 1, except that no additive is used in the preparation of component B.
[0119] The following tests were conducted using the polishing compositions or polishing liquids of the above examples and comparative examples.
[0120] (1) The test method of SOD material removal rate includes: providing a plurality of identical first test wafers, each of which includes a blank wafer and a SOD material layer formed on the blank wafer. Then, under the same test conditions, polishing the SOD material layers on the plurality of first test wafers is performed using a polishing machine, the polishing composition or the polishing liquid of the embodiment and the comparative example, respectively, to obtain the removal rate of the SOD material layer by the polishing composition or the polishing liquid of the embodiment and the comparative example.
[0121] (2) The method for testing the silicon nitride material removal rate includes: providing a plurality of identical second test wafers, each of which includes a blank wafer and a silicon nitride layer formed on the blank wafer. Then, under the same test conditions, polishing the plurality of second test wafers is performed using a polishing machine, the polishing composition or polishing liquid of the embodiment and the comparative example, respectively, to obtain the removal rate of the silicon nitride layer by the polishing composition or polishing liquid of the embodiment and the comparative example.
[0122] (3) A method for testing the polishing time of a product wafer comprises: providing a plurality of identical product wafers, wherein the product wafers include a SOD material layer and a silicon nitride pattern formed by a photolithography process; polishing the plurality of product wafers respectively using a polishing machine, and the polishing composition or polishing liquid of the embodiment and the comparative example, to obtain the polishing time of the product wafers by the polishing composition or polishing liquid of the embodiment and the comparative example.
[0123] (4) Auto position inspection (API) defect inspection, using an automatic position inspection device to obtain defects of the product wafer after polishing in the above product wafer polishing time test. If the silicon nitride pattern on the product wafer is intact, the API defect inspection passes, which is indicated by OK. On the contrary, if the silicon nitride pattern on the product wafer is not intact, the API defect inspection fails, which is indicated by NG.
[0124] The polishing machine is an AMAT-LKP CMP polishing machine produced by Applied Materials. The same test conditions include the same grinding time, the rotation speed of the polishing machine and the grinding pressure.
[0125] Table 1
[0126]
[0127]
[0128] Combining Examples 1 to 5 and Comparative Examples 1 to 5, it can be seen that under the same process conditions, the polishing compositions of Examples 1 to 5 prepared with two components can reduce grinding defects on the product wafer during the polishing process and improve the planarization effect.
[0129] In combination with Examples 1 to 5 and Comparative Examples 1 to 3, it can be seen that the polishing composition of Examples 1 to 5 prepared using two components has a shorter polishing time for the product sheet and a greater removal selectivity for the SOD material layer / silicon nitride layer, indicating that the polishing composition of the present application has a higher polishing rate and a greater selectivity for the SOD material.
[0130] and, Figure 2 BSL is a partial schematic diagram of wafer C and wafer E after being treated by the polishing liquid of comparative example 1. Figure 2 Mix slurry-X is a partial schematic diagram of the polishing composition of Example 1 after processing wafer C and wafer E. Figure 2 It can be seen that under the same process conditions, the polishing composition of Example 1 prepared by using two components can effectively improve the over-polishing defects inside the wafer.
[0131] also, Figure 3 BSL is a partial schematic diagram of the silicon nitride layer pattern of the cut line after the wafer is processed by the polishing liquid of Comparative Example 1. Figure 3 Mix slurry-X is a partial schematic diagram of the silicon nitride layer pattern of the cut street after the wafer is processed by the polishing composition of Example 1. For low-density patterns, medium-density patterns, and high-density patterns, the distribution density of the patterns increases. Figure 3 It can be seen that under the same process conditions, the polishing composition of Example 1 prepared by using two components can effectively improve the over-polishing defect of the silicon nitride layer pattern with different densities at the cutting street.
[0132] The description of the above embodiments is only used to help understand the technical solutions and core ideas of the present application. Ordinary technical personnel in this field should understand that they can still modify the technical solutions recorded in the aforementioned embodiments, or replace some of the technical features therein with equivalents. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present application.
Claims
1. A polishing composition for polishing an organic dielectric layer, characterized in that: The invention comprises component A and component B. The component A is an abrasive solution, and the component B comprises a surfactant and an additive, wherein the additive is 4-hydroxybenzoic acid.
2. The polishing composition for polishing an organic dielectric layer according to claim 1, characterized in that: Calculated by mass percentage, the B component includes the following components:
3. The polishing composition for polishing an organic dielectric layer according to claim 2, characterized in that: In the B component, the mass ratio of the surfactant to the additive is (0.6-1.5):
1.
4. The polishing composition for polishing an organic dielectric layer according to claim 2, characterized in that: The first pH regulator is selected from at least one of an organic acid and an organic base; and / or, The surfactant is selected from at least one of fatty alcohol polyoxyethylene ether, fatty acid polyoxyethylene ester and alkylphenol polyoxyethylene ether; and / or, The B component is an acidic solution.
5. The polishing composition for polishing an organic medium layer according to claim 1, characterized in that: Calculated by mass percentage, the A component includes the following components:
6. The polishing composition for polishing an organic dielectric layer according to claim 5, characterized in that: The abrasive is ceria sol, the solid content of the ceria sol is 5% to 40%; and / or the particle size of the ceria sol is 150nm to 350nm; and / or, The dispersant is methyl amyl alcohol; and / or, The chelating agent is at least one selected from FA / O chelating agent, tetrahydroxyethylethylenediamine, ethylenediamine and triethanolamine; and / or, The second pH regulator is selected from at least one of an organic acid and an organic base; and / or, The A component is an acidic solution.
7. The polishing composition for polishing an organic dielectric layer according to claim 1, characterized in that: The polishing composition comprises: Component A: 20 wt% to 50 wt%; Component B 8wt% to 15wt%; and Water, balance.
8. The polishing composition for polishing an organic dielectric layer according to claim 1, characterized in that: The pH value of the polishing composition is an acidic solution.
9. The polishing composition for polishing an organic dielectric layer according to claim 1, characterized in that: The organic medium layer includes a C element.
10. A method for manufacturing a semiconductor device, characterized in that: The steps include: Providing the component A according to any one of claims 1 to 9 and the component B, and mixing the two to obtain a polishing composition for polishing an organic medium layer; Providing a semiconductor structure, the semiconductor structure comprising an organic dielectric layer and an inorganic layer, wherein the organic dielectric layer covers the inorganic layer; as well as A polishing pad and the polishing composition are used to remove a portion of the organic medium layer until the inorganic layer is exposed, thereby obtaining a polished organic medium layer.