Water-based lithium ion battery silicon-carbon negative electrode binder and application thereof
By extracting water-soluble paint polysaccharide and polyacrylonitrile from raw paint, the silicon carbon negative electrode binder of water-based lithium-ion batteries is prepared, which solves the problem of easy falling off of silicon carbon materials in lithium-ion batteries, and significantly improves the cycle stability of the battery and electrochemical properties.
Patent Information
- Application Number
- CN202411376975.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-11-22
AI Technical Summary
The silicon carbon material in lithium-ion batteries is prone to pulverization and fall off due to volume expansion during charging and discharging, resulting in rapid attenuation of battery capacity. In addition, existing water-based adhesives are insufficiently developed, making it difficult to improve battery cycle stability.
By isolating water-soluble lacquer polysaccharide (LPS) from the raw lacquer residue after extracting uluol, compounded with the traditional binder polyacrylonitrile (PAN), it is used as a silicon carbon negative electrode binder for aqueous lithium-ion batteries, and combined with vapor-phase deposition of silicon Carbon and conductive carbon are used to prepare negative electrode materials by ball milling.
It significantly improves the battery life and electrical cycling performance of lithium-ion batteries, enhances the discharge capacity and charge and discharge efficiency at room temperature and low temperature, and extends the battery life.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to an aqueous silicon-carbon negative electrode binder for lithium ion batteries and application thereof. Background Art
[0002] High specific capacity silicon-carbon materials are considered to be the most promising negative electrode materials for lithium-ion batteries. However, the volume expansion effect of silicon during the charge / discharge process causes the electrode materials to be easily crushed and detached, which can easily cause the battery capacity to decay rapidly. Therefore, it is particularly important to develop reliable silicon-carbon negative electrode binders to improve battery cycle stability.
[0003] In recent years, under the guidance of environmental protection concepts and sustainable development strategies, water-based binders have been favored by researchers due to their advantages of being green, pollution-free and having strong adhesiveness. Raw lacquer is a high-quality natural product resource with Chinese characteristics. After extracting lacquer phenol from raw lacquer, the remaining residue accounts for 25-30% of the total mass, and the main components are gum, lacquer polysaccharide and laccase. Due to the complex mixture of these components, it is difficult to purify them to obtain a pure single component and they are often ignored by researchers or even directly discarded, which causes a serious waste of resources. The present invention separates the insoluble substances in the ethanol solvent after extracting lacquer phenol from raw lacquer to obtain water-soluble lacquer polysaccharide (LPS), which is used as a binder in lithium-ion batteries, and preliminarily explores the effect of water-soluble lacquer polysaccharide as a binder on the electrochemical properties of the electrode. Summary of the invention
[0004] The object of the present invention is to provide an aqueous lithium-ion battery silicon-carbon negative electrode binder and its application to solve the problems raised in the above background technology.
[0005] In order to solve the above technical problems, the first aspect of the present invention provides the following technical solutions: A water-based lithium-ion battery silicon-carbon negative electrode binder, which includes water-soluble lacquer polysaccharide (LPS).
[0006] Furthermore, the LPS is extracted from the raw lacquer residue after extracting lacquer phenol; the specific extraction process is: (1) placing the raw lacquer residue after extracting lacquer phenol in a cool and dry place, and after the ethanol evaporates, a solid residue is obtained; (2) the solid residue and deionized water are mixed and stirred at a mass ratio of 1:1 for 12 to 36 hours, and then the vacuum filtration is repeated 3 to 4 times, and finally the filtrate is dried to obtain LPS.
[0007] Furthermore, the aqueous lithium-ion battery silicon-carbon negative electrode binder also includes a traditional binder.
[0008] Furthermore, the conventional binder includes but is not limited to polyacrylonitrile (PAN).
[0009] Furthermore, the composite mass ratio of LPS and PAN is (1~3):(1~3).
[0010] Furthermore, the composite mass ratio of LPS and PAN is 1:1 or 1:3 or 3:1.
[0011] Furthermore, the PAN model is Tinctive E124, hereinafter referred to as E124.
[0012] PAN has a large number of electron-withdrawing groups -CN, which can form strong hydrogen bonds with the bonded substances through hydrogen bonds and dipole-dipole effects, making the bonds tighter. Therefore, it is often used as an electrode binder.
[0013] The second aspect of the present invention proposes the application of the aqueous lithium-ion battery silicon-carbon negative electrode binder, which is characterized in that: vapor-deposited silicon carbon, conductive carbon (Super-P), and the aqueous lithium-ion battery silicon-carbon negative electrode binder are added to a ball mill in a mass ratio of 3:1:1, and ball milled at a speed of 150r / min, and N-methylpyrrolidone (NMP) is added in small amounts and multiple times until the mixture becomes viscous, and finally ball milled at a speed of 200r / min for 2h to obtain a slurry, which is coated on an aluminum foil to be processed into a negative electrode.
[0014] Compared with the prior art, the beneficial effects achieved by the present invention are: (1) LPS can improve the bonding performance of the binder, prevent the active material from peeling off from the current collector aluminum foil during long cycles, and greatly improve the battery life and electrical cycle performance of lithium-ion batteries; (2) The present invention improves the electrochemical performance of lithium-ion batteries, especially the discharge capacity, charge and discharge efficiency and capacity retention rate at room temperature and low temperature. DETAILED DESCRIPTION
[0015] The following is a preferred implementation of the embodiment of the present invention. Obviously, the described embodiment is only a part of the embodiment of the present invention, not all of the embodiments. For ordinary technicians in this technical field, all other embodiments obtained by ordinary technicians in this field without creative work without departing from the principle of the embodiment of the present invention are within the scope of protection of the present invention.
[0016] In the following examples, all raw materials come from the following sources: Raw lacquer, vapor-deposited silicon carbon, and conductive carbon (Super-P) were purchased from Shenzhen Kejing Zhida Technology Co., Ltd.; NMP and PVDF were purchased from Aladdin (Shanghai) Reagent Network; Nickel-cobalt-manganese ternary cathode material (NCM811), electrolyte (TC-E8630E3), and Tinctive E124 were all purchased from Tianci High-tech Materials Co., Ltd.
[0017] Example 1: A water-based lithium-ion battery silicon-carbon negative electrode binder: Step 1: (1) Place the raw lacquer residue after extracting lacquer phenol in a cool and dry place, and after the ethanol evaporates, obtain a solid residue; (2) Mix the solid residue and deionized water in a mass ratio of 1:1 and stir for 24 hours, repeat the vacuum filtration 4 times, and finally dry the filtrate to obtain an aqueous lithium-ion battery silicon-carbon negative electrode binder (LPS).
[0018] Based on Example 1, Examples 2 to 4 are set: Example 2: Example 2 is based on Example 1, except that LPS is compounded with E124, and other processes remain unchanged, specifically: Step 2: Mix LPS and E124 in a mass ratio of 1:1 to obtain an aqueous lithium-ion battery silicon-carbon negative electrode binder (LPS / E124-1).
[0019] Example 3: Example 3 is based on Example 1, except that LPS is compounded with E124, other processes remain unchanged, specifically: Step 2: Mix LPS and E124 in a mass ratio of 1:3 to obtain an aqueous lithium-ion battery silicon-carbon negative electrode binder (LPS / E124-2).
[0020] Example 4: Example 4 is based on Example 1, except that LPS is compounded with E124, and other processes remain unchanged, specifically: Step 2: Mix LPS and E124 in a mass ratio of 3:1 to obtain an aqueous lithium-ion battery silicon-carbon negative electrode binder (LPS / E124-3).
[0021] Based on Example 1, a control experiment is carried out to set comparative examples 1 to 3; based on Example 2, a control experiment is carried out to set comparative example 4, which is specifically described as follows: Comparative Example 1: Comparative Example 1 is based on Example 1, with the following modifications: using a conventional binder, polyvinylidene fluoride (PVDF), as a binder for the silicon-carbon negative electrode of an aqueous lithium-ion battery (PVDF is a semi-crystalline polymer, and its high crystallinity gives it a high bonding force, which can tightly bind the bonded materials, and is therefore often used as an electrode binder); Comparative Example 2: Comparative Example 2 is based on Example 1, using LPS and PVDF compounding, and other processes remain unchanged, specifically: Step 2: Mix LPS and PVDF in a mass ratio of 1:1 to obtain an aqueous lithium-ion battery silicon-carbon negative electrode binder (LPS / PVDF-1).
[0022] Comparative Example 3: Comparative Example 3 is based on Example 1, using LPS and PVDF compounding, and other processes remain unchanged, specifically: Step 2: Mix LPS and PVDF in a mass ratio of 3:1 to obtain an aqueous lithium-ion battery silicon-carbon negative electrode binder (LPS / PVDF-2).
[0023] Comparative Example 4: Comparative Example 4 is based on Example 2, with the following adjustments: only E124 is used as the aqueous lithium-ion battery silicon-carbon negative electrode binder.
[0024] Performance test: The performance test of the aqueous lithium-ion battery silicon-carbon negative electrode binder corresponding to Examples 1 to 4 and Comparative Examples 1 to 4 was performed, and the specific test was as follows: (1) Vapor-deposited silicon carbon, Super-P, binders corresponding to Examples 1 to 4 and Comparative Examples 1 to 4 were added to a ball mill at a mass ratio of 3:1:1, and ball milled at a speed of 150 r / min. NMP was added in small amounts and multiple times until the mixture became viscous. Finally, the mixture was ball milled at a speed of 200 r / min for 2 h to obtain a slurry, which was coated on an aluminum foil with a coating thickness of 100 μm and dried at 60° C. for 24 h to obtain a negative electrode sheet, ensuring that the average loading of the active material in the negative electrode sheet was 0.8 mg / cm 2 (2) Cutting the negative electrode sheet into circular electrode sheets with a diameter of 14 mm by a punching machine, assembling the circular negative electrode sheet and a positive electrode sheet of model NCM811 into a button half-cell, injecting an electrolyte of model TC-E8630E3 into the button cell to obtain a button cell.
[0025] At 25°C, the peeling force of the button cell corresponding to each example and the discharge capacity after 100 charge and discharge cycles at a current density of 4A / g were tested respectively; the peeling force test method is as follows: 1. Peel force test: (1) Stick one side of the 3M-VHB double-sided tape on the negative electrode of the button battery and the other side on the stainless steel plate. The three are integrated into one. (2) Fix the whole on the two clamps of the peel force tester and perform a 180° peel test at a speed of 10 mm / min until the negative electrode sheet is completely peeled off.
[0026] The specific data are shown in Table 1 below:
[0027] Result analysis: From the data in Table 1 above, it can be seen that LPS, as a new type of silicon-carbon negative electrode binder, can well replace the traditional binder PVDF, so that the battery exhibits good peeling force and electrical cycling ability. Compared with PVDF, its performance improvement is more obvious; by compounding LPS and PAN (Tinctive E124), the nitrile group in PAN can form strong hydrogen bonds with the bonded material through hydrogen bonds and bipolar-dipole effects. The synergy of the two can greatly improve the peeling force and enhance the electrical cycling performance. When the mass ratio of LPS to E124 is 3:1, the optimal performance is achieved.
[0028] Finally, it should be noted that the above is only a preferred embodiment of the present invention, but the protection scope of this application is not limited thereto. Any changes or substitutions that can be easily thought of by any technician familiar with the technical field within the spirit and principle of the present invention and within the technical scope disclosed in this application should be included in the protection scope of this application; in the absence of conflict, the embodiments of this application and the features in the embodiments can be combined with each other. Therefore, the protection scope of this application shall be based on the protection scope of the claims.
Claims
1. A water-based silicon-carbon negative electrode binder for lithium-ion batteries, Features: The aqueous lithium-ion battery silicon-carbon negative electrode binder includes water-soluble lacquer polysaccharide; The water-soluble lacquer polysaccharide is extracted from the raw lacquer residue after lacquer phenol is extracted.
2. The aqueous silicon-carbon negative electrode binder for lithium-ion batteries according to claim 1, Features: The extraction process of the water-soluble lacquer polysaccharide is specifically as follows: (1) placing the raw lacquer residue after extracting urushiol in a cool place to dry, and removing ethanol to obtain a solid residue; (2) The solid residue is mixed with deionized water, and the mixture is repeatedly filtered under reduced pressure, and the filtrate is finally dried to obtain water-soluble lacquer polysaccharide.
3. The aqueous silicon-carbon negative electrode binder for lithium-ion batteries according to claim 1, Features: The aqueous lithium-ion battery silicon-carbon negative electrode binder also includes a traditional binder.
4. The aqueous silicon-carbon negative electrode binder for lithium-ion batteries according to claim 3, Features: The conventional binder includes polyacrylonitrile.
5. The aqueous silicon-carbon negative electrode binder for lithium-ion batteries according to claim 3, Features: The composite mass ratio of the water-soluble lacquer polysaccharide and the traditional binder is (1-3):(1-3).
6. The aqueous silicon-carbon negative electrode binder for lithium-ion batteries according to claim 5, Features: The compounding mass ratio of the water-soluble lacquer polysaccharide and the traditional binder is 1:1 or 1:3 or 3:
1.
7. The aqueous silicon-carbon negative electrode binder for lithium-ion batteries according to claim 4, Features: The polyacrylonitrile model is Tinctive E124.
8. Use of an aqueous silicon-carbon negative electrode binder for lithium-ion batteries according to any one of claims 1 to 7, Features: The vapor-deposited silicon carbon, conductive carbon, the aqueous lithium-ion battery silicon-carbon negative electrode binder and the solvent are ball-milled to obtain a slurry, which is then coated on an aluminum foil to prepare a lithium-ion battery silicon-carbon negative electrode.
9. Application of an aqueous silicon-carbon negative electrode binder for lithium-ion batteries according to claim 8, Features: The mass ratio of the vapor deposited silicon carbon, the conductive carbon and the aqueous lithium ion battery silicon carbon negative electrode binder is 3:1:1.