Bio-based cobalt salt tackifying belt compound and preparation method thereof

By using renewable bio-based cobalt salts to replace cobalt boronylides in the belt layer glue, the adhesion between rubber and steel cords is improved, and the problem of insufficient adhesion performance in the prior art is solved and the service life of the tire is extended And reduce production costs.

CN118995082APending Publication Date: 2024-11-22DOUBLE COIN GRP (CHONGQING) TIRE CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410907893.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In the prior art, the adhesive performance between rubber and steel cords is insufficient, resulting in a shortening of the service life of the tire, and the excessive use of cobalt salt increases production costs, affecting the aging resistance.

Method used

Replace cobalt boronacylated as a new adhesive by regenerating bio-based cobalt salts, improving the adhesion between rubber and steel cords by modifying adhesive resins and bio-based materials, reducing the amount of cobalt, and combining with specific mixing The process and formula are composed to form an efficient belt adhesive.

Benefits of technology

The adhesive force, tensile strength and tear-break elongation of the belt adhesive are improved, the compression heat generation temperature is reduced, the service life of the tire is extended, and the production cost is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118995082A_ABST
    Figure CN118995082A_ABST
Patent Text Reader

Abstract

The invention relates to a bio-based cobalt salt tackified belt compound and a preparation method thereof.The belt compound is prepared from, by mass, 80-100 parts of natural rubber, 5-10 parts of white carbon black, 40-55 parts of carbon black, 6-10 parts of zinc oxide, 0-1 part of stearic acid, 0.5-2 parts of accelerant, 1-3 parts of anti-aging agent RD, 2-4 parts of anti-aging agent 4020, 0.5-1.5 parts of bio-based cobalt salt and 0-1 part of tackifying resin. 0-3 parts of modified bonding resin, 2-6 parts of sulfur and 0-0.5 part of scorch retarder. Compared with the prior art, the prepared belted layer rubber has excellent bonding performance and aging resistance, cobalt boroacylate is replaced with the cobalt salt (bio-based cobalt salt for short) modified by the renewable rubber compatilizer, the consumption of the cobalt salt in the rubber material is reduced, the bonding performance and aging resistance of the belted layer rubber material are improved, and the service life of the belted layer rubber material is prolonged. Therefore, the service life of the tire is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of chemical materials, and in particular to a bio-based cobalt salt tackifying belt layer adhesive and a preparation method thereof. Background Art

[0002] In recent years, the state has placed increasingly high demands on enterprises for environmental protection. At present, there have been some studies on bio-based plastics, bio-based rubbers, and bio-based material additives to solve the problems of fossil energy shortage and environmental pollution. Bio-based material-rubber compatibilizer refers to "zero carbon" or "negative carbon" materials obtained through biomanufacturing or chemical processing using biomass as raw materials. Among them, biomass refers to various organisms formed through photosynthesis, including materials derived from all living organisms such as animals, plants, and microorganisms. Lignin is one of the important components of rubber compatibilizers. It is the second largest natural organic polymer compound in plants after cellulose. It is a bio-based material with excellent corrosion resistance, heat resistance, and antioxidant properties. Extracting lignin from straw can also help improve the utilization rate of crops.

[0003] Among tire components, the belt layer mainly constrains and maintains the shape of the tire crown, and it bears 60% to 70% of the internal stress of the tire. As the main skeleton material of the tire belt layer, it is crucial to explore the factors affecting the adhesion performance between rubber and steel cord for the development of the rubber industry. The adhesion between rubber and steel cord is directly related to the service life of the tire. However, rubber and steel cord are two completely different substances. They need to be well bonded together under certain conditions and have the characteristics of both. Cobalt borate is a good adhesion promoter, which is beneficial to improve the adhesion between rubber and steel cord. However, cobalt is an expensive material, and the amount of cobalt used in rubber is too high, which is not conducive to the aging resistance of the tire. Summary of the invention

[0004] The purpose of the present invention is to provide a bio-based cobalt salt tackifying belt layer rubber and a preparation method thereof in order to solve the above-mentioned problems. The present invention adopts cobalt borate modified by a renewable rubber compatibilizer as a new type of bio-based adhesive to replace the cobalt borate in the belt layer rubber in an equal amount, thereby reducing the amount of cobalt used and saving production costs.

[0005] The purpose of the present invention is achieved through the following technical solutions:

[0006] The first object of the present invention is to provide a bio-based cobalt salt tackified belt layer adhesive, wherein the bio-based cobalt salt tackified belt layer adhesive comprises the following components in parts by weight:

[0007]

[0008] Furthermore, the carbon black is N326 carbon black.

[0009] Furthermore, the tackifying resin is WDH-B resin.

[0010] Furthermore, the modified adhesive resin is SL-3022 resin.

[0011] Furthermore, the bio-based cobalt salt tackifying belt layer adhesive further comprises the following components in parts by weight:

[0012] 0.5 to 1.5 parts of cobalt borate.

[0013] Furthermore, the bio-based cobalt salt tackifying belt layer adhesive further comprises the following components in parts by weight:

[0014] Adhesive 0-5 parts.

[0015] Furthermore, the adhesive is adhesive RA-65.

[0016] Furthermore, the promoter is promoter NS.

[0017] Furthermore, the anti-scorching agent is anti-scorching agent CTP.

[0018] Furthermore, the sulfur is insoluble sulfur.

[0019] Furthermore, in the formula, the content of natural rubber does not exceed 100 parts by weight, and the total content of other raw materials is lower than the content of natural rubber.

[0020] The invention uses renewable bio-based cobalt salt to replace cobalt boroacylate, so that the rubber and the steel wire have better adhesion, and can improve the 300% tensile stress, tensile strength and elongation at break of the rubber compound.

[0021] The second object of the present invention is to provide a method for preparing the above-mentioned bio-based cobalt salt tackifying belt layer adhesive, comprising the following preparation steps:

[0022] S1. In the mixing chamber of the internal mixer, add natural rubber, mix for 30 seconds and then remove the top plug, add white carbon black and mix for 28 seconds and then remove the top plug, mix until the temperature reaches 164°C and the rubber is discharged to obtain a masterbatch;

[0023] S2. In the mixing chamber of the internal mixer, add masterbatch, carbon black, zinc oxide, stearic acid, and antioxidant RD, mix for 22 seconds, and then remove the top plug. Add tackifying resin and bio-based cobalt salt, mix for 25 seconds, and then remove the top plug. Reduce the speed to 30 rpm, and mix until the temperature reaches 165°C for rubber removal. This rubber is a first-stage mixed rubber.

[0024] S3. Add the first-stage mixed rubber, antioxidant 4020 and zinc oxide into the mixing chamber of the internal mixer, mix for 10 seconds, lift the top bolt, reduce the speed to 30 rpm, mix until the temperature reaches 147°C and discharge the rubber. This rubber is the second-stage mixed rubber.

[0025] S4. After the second-stage mixed rubber is parked for 12 hours, it is sulfurized and finally refined. The second mixed rubber, sulfur, accelerator, adhesive and anti-scorch agent are put into the mixing chamber of the internal mixer. Mix for 25 seconds, lift the top plug, stay for 3 seconds, press the plug, reduce the speed to 15rpm, mix to a temperature of 101℃, lift the plug and discharge the rubber to obtain the finished product, which is the bio-based cobalt salt tackified belt layer rubber.

[0026] Furthermore, in step S1, the conditions of the internal mixer are as follows: the rotor speed of the internal mixer is 50 rpm, the mixing pressure is 5 MPa, the cooling water temperature is 35°C, and the rotor temperature is 35°C.

[0027] Further, in step S2, the conditions of the internal mixer are as follows: the rotor speed of the internal mixer is 50 rpm, the mixing pressure is 6 MPa, the cooling water temperature is 35° C., and the rotor temperature is 35° C.;

[0028] Further, in step S3, the conditions of the internal mixer are as follows: the rotor speed of the internal mixer is 50 rpm, the mixing pressure is 6 MPa, the cooling water temperature is 35° C., and the rotor temperature is 35° C.;

[0029] Furthermore, in step S4, the conditions of the internal mixer are as follows: the rotor speed of the internal mixer is 30 rpm, the mixing pressure is 4.5 MPa, the cooling water temperature is 30°C, and the rotor temperature is 30°C.

[0030] Compared with the prior art, the beneficial effects of the present invention are embodied in the following aspects:

[0031] 1) The bio-based cobalt salt tackifying belt layer adhesive of the present technical solution improves the adhesion of the belt layer formula by using a new type of bio-based adhesive, and also increases the tensile strength and elongation at break, and reduces the compression heat generation temperature.

[0032] 2) The bio-based cobalt salt tackifying belt layer rubber of the present technical solution uses renewable bio-based cobalt salt to replace cobalt borate to achieve better adhesion between rubber and steel wire, thereby improving the 300% tensile stress, tensile strength and elongation at break of the rubber compound.

[0033] 3) The belt layer in the tire is the transition from the tread to the carcass, which plays a role in mitigating impact force and protecting the carcass. Its main performance requirements include high metal adhesion, high elongation, aging resistance, low heat generation, etc. Although cobalt salt is beneficial to the bonding between rubber and steel wire, it cannot achieve the ideal bonding effect if the dosage is improper. If the dosage is too low, the bonding strength will not meet the requirements; if the dosage is too high, the bonding retention rate between the steel wire and the rubber after aging will be greatly reduced, and it will also cause dezincification and reduce the service life of the tire. The new bio-based modified cobalt salt used in the present invention retains 70% of the main amount of cobalt borate, reducing the amount of cobalt borate. Bio-based materials improve the compatibility between adhesives and rubber, and the surface activation of bio-based materials is also conducive to the formation of Cu with adhesion. x S layer. Maintaining the optimal amount of cobalt borate body can not only improve tire quality and extend tire service life, but also keep product costs low, creating significant economic benefits for the company. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 It is a schematic diagram of the adhesion of the bio-based cobalt salt tackified belt adhesive of the embodiment and the belt adhesive of the control example before and after heat aging. DETAILED DESCRIPTION

[0035] The present invention is described in detail below in conjunction with specific embodiments, but is by no means intended to limit the present invention. Features such as preparation methods, materials, structures or composition ratios not explicitly described in this technical solution are considered to be common technical features disclosed in the prior art.

[0036] In the following examples and comparative examples, natural rubber was purchased from GSR9710 of Yunnan Dianyuan Rubber International Trade Co., Ltd.; white carbon black was purchased from Quecheng Silicon Chemical Co., Ltd.; carbon black N326 was purchased from Zhongxiang (Chongqing) Carbon Black Co., Ltd.; zinc oxide was purchased from Chongqing Judu Zinc Co., Ltd.; stearic acid was purchased from Nantong Kaita Chemical Technology Co., Ltd.; antioxidant 4020 was purchased from Kemai Chemical Co., Ltd.; antioxidant RD was purchased from Kemai Chemical Co., Ltd.; cobalt borate was purchased from Jiangyin Sanliang Rubber and Plastic New Materials Co., Ltd.; bio-based cobalt salt was purchased from Qingdao Zhongke Heyuan New Materials Co., Ltd. The model is modified cobalt borate-70 (including 70wt% cobalt borate and 30wt% bio-based materials, and the bio-based materials are mainly obtained by methylation modification and compatibility modification of lignin); WDH-B resin was purchased from Wuhan Jinghe Chemical (Qianjiang) Co., Ltd.; SL-3022 resin was purchased from Huaqi (China) Chemical Co., Ltd.; RA-65 adhesive was purchased from Jiangsu Guoli Chemical Technology Co., Ltd.; accelerator NS was purchased from Kemai Chemical Co., Ltd.; sulfur was purchased from Jiangsu Hongtai Rubber Additives Co., Ltd.; anti-scorch agent CTP was purchased from Shandong Yanggu Huatai Chemical Co., Ltd.

[0037] Example

[0038] The components and weight proportions of the bio-based cobalt salt tackifying belt layer adhesive in this embodiment are shown in Table 1.

[0039] The preparation method of the bio-based cobalt salt tackifying belt layer rubber in this embodiment adopts a masterbatch, first stage, second stage and final mixing process, which includes the following steps:

[0040] Masterbatch plasticizing: set the rotor speed of the internal mixer to 50rpm, the mixing pressure to 5MPa, the cooling water temperature to 35℃, the rotor temperature to 35℃, add natural rubber, mix for 30 seconds and lift the top plug, add white carbon black, mix for 28 seconds and lift the top plug, mix until the temperature reaches 164℃ and discharge the rubber to obtain the masterbatch;

[0041] One-stage mixing: set the rotor speed of the internal mixer to 50rpm, the mixing pressure to 6MPa, the cooling water temperature to 35℃, the rotor temperature to 35℃, add masterbatch, carbon black N326, zinc oxide (60% of the total amount), stearic acid, antioxidant RD, mix for 22 seconds and lift the top plug, add WDH-B resin and bio-based cobalt salt, mix for 25 seconds and lift the top plug, reduce the speed to 30rpm, mix until the temperature reaches 165℃ and discharge, this rubber is a one-stage mixed rubber;

[0042] Second stage mixing: start the internal mixer, set the rotor speed of the internal mixer to 50rpm, the mixing pressure to 6MPa, the cooling water temperature to 35℃, the rotor temperature to 35℃, add the first stage mixed rubber, antioxidant 4020, zinc oxide (40% of the total amount), mix for 10 seconds, lift the top bolt, reduce the speed to 30rpm, mix until the temperature reaches 147℃ and discharge the rubber, this rubber is the second stage mixed rubber;

[0043] The second stage mixed rubber is left standing for 12 hours before adding sulfur and final refining;

[0044] Final refining: Start the internal mixer, set the rotor speed of the internal mixer to 30rpm, the mixing pressure to 4.5MPa, the cooling water temperature to 30℃, the rotor temperature to 30℃, put the second mixed rubber and sulfur, accelerator NS, adhesive RA-65 and anti-scorch agent CTP into the mixing chamber, mix for 25 seconds, lift the top plug, stay for 3 seconds, press the plug, reduce the speed to 15rpm, mix to a temperature of 101℃, lift the plug and discharge the glue to obtain the finished bio-based cobalt salt tackified belt layer rubber.

[0045] The physical properties of the finished bio-based cobalt salt tackifying belt layer adhesive are shown in Figure 2. Figure 1 .

[0046] Comparison Example

[0047] The components and weight proportions of the belt layer adhesive in this comparative example are shown in Table 1.

[0048] The preparation method of the belt layer rubber in this comparative example adopts a masterbatch, first stage, second stage and final mixing process, which is basically the same as the embodiment, except that: cobalt borate is added in the first stage mixing instead of bio-based cobalt salt.

[0049] The physical properties of the belt layer rubber are shown in Figure 2. Figure 1 .

[0050] Table 1. Examples of formulations.

[0051]

[0052]

[0053] Table 2 Physical properties of embodiments and control examples.

[0054]

[0055]

[0056] It can be seen from Table 2 that compared with the control example formulation, the Mooney viscosity of the embodiment formulation is slightly increased and the scorch time is shortened, but overall the effect on the processing performance of the rubber compound is small. H It is only reduced by 1.9, the vulcanization rate is the same, the 300% tensile stress, tensile strength and elongation at break are better than the control formula, and other physical properties are the same. After the adhesion promoter in the belt layer rubber is replaced with bio-based cobalt salt, the compression heat generation temperature of the rubber is reduced by 4.8℃ compared with the control formula, which is beneficial to improve the service life of the tire.

[0057] Figure 1 The results show that the bonding performance of the embodiment formula before aging is better than that of the control formula. This is because the appropriate amount of rubber compatibilizer improves the compatibility between substances, reduces the repulsive force between cobalt and non-polar rubber molecules, improves the interface reaction of rubber / steel cord, and is conducive to the formation of Cu with adhesion. x S. After the bio-based cobalt salt replaced the cobalt borate, the bonding performance of the example formula after 24h and 48h heat aging was better, which may be because the bio-based material reduced the dezincification effect in the bonding interface. The bonding retention rate of the example formula after aging was better and the aging resistance was improved, which was related to the good aging resistance of lignin in the bio-based cobalt salt (the bio-based material in the bio-based cobalt salt is mainly modified from lignin).

[0058] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. A bio-based cobalt salt tackifying belt layer rubber, characterized in that: The bio-based cobalt salt tackifying belt layer adhesive comprises the following components in parts by weight:

2. The bio-based cobalt salt tackifying belt adhesive according to claim 1, characterized in that: The carbon black is N326 carbon black.

3. The bio-based cobalt salt tackifying belt adhesive according to claim 1, characterized in that: The tackifying resin is WDH-B resin.

4. The bio-based cobalt salt tackifying belt adhesive according to claim 1, characterized in that: The modified adhesive resin is SL-3022 resin.

5. The bio-based cobalt salt tackifying belt adhesive according to claim 1, characterized in that: The bio-based cobalt salt tackifying belt layer adhesive further comprises the following components in parts by weight: 0.5-1.5 parts of cobalt boroacylate; Adhesive 0-5 parts.

6. The bio-based cobalt salt tackifying belt adhesive according to claim 5, characterized in that: The adhesive is adhesive RA-65.

7. The bio-based cobalt salt tackifying belt adhesive according to claim 1, characterized in that: The accelerator is accelerator NS.

8. The bio-based cobalt salt tackifying belt adhesive according to claim 1, characterized in that: The anti-scorching agent is anti-scorching agent CTP.

9. A method for preparing the bio-based cobalt salt tackifying belt layer adhesive as claimed in any one of claims 1 to 8, characterized in that: The method comprises the following steps: S1. In the mixing chamber of the internal mixer, add natural rubber, mix for 30 seconds and then remove the top plug, add white carbon black and mix for 28 seconds and then remove the top plug, mix until the temperature reaches 164°C and the rubber is discharged to obtain a masterbatch; S2. In the mixing chamber of the internal mixer, add masterbatch, carbon black, zinc oxide, stearic acid, and antioxidant RD, mix for 22 seconds, and then remove the top plug. Add tackifying resin and bio-based cobalt salt, mix for 25 seconds, and then remove the top plug. Reduce the speed to 30 rpm, and mix until the temperature reaches 165°C for rubber removal. This rubber is a first-stage mixed rubber. S3. Add the first-stage mixed rubber, antioxidant 4020 and zinc oxide into the mixing chamber of the internal mixer, mix for 10 seconds, lift the top bolt, reduce the speed to 30 rpm, mix until the temperature reaches 147°C and discharge the rubber. This rubber is the second-stage mixed rubber. S4. After the second-stage mixed rubber is parked for 12 hours, it is sulfurized and finally refined. The second mixed rubber, sulfur, accelerator, adhesive and anti-scorch agent are put into the mixing chamber of the internal mixer. Mix for 25 seconds, lift the top plug, stay for 3 seconds, press the plug, reduce the speed to 15rpm, mix to a temperature of 101℃, lift the plug and discharge the rubber to obtain the finished product, which is the bio-based cobalt salt tackified belt layer rubber.

10. The method for preparing a bio-based cobalt salt tackifying belt adhesive according to claim 9, characterized in that: In step S1, the conditions of the internal mixer are as follows: the rotor speed of the internal mixer is 50 rpm, the mixing pressure is 5 MPa, the cooling water temperature is 35° C., and the rotor temperature is 35° C.; In step S2, the conditions of the internal mixer are as follows: the rotor speed of the internal mixer is 50 rpm, the mixing pressure is 6 MPa, the cooling water temperature is 35° C., and the rotor temperature is 35° C.; In step S3, the conditions of the internal mixer are as follows: the rotor speed of the internal mixer is 50 rpm, the mixing pressure is 6 MPa, the cooling water temperature is 35° C., and the rotor temperature is 35° C.; In step S4, the conditions of the internal mixer are as follows: the rotor speed of the internal mixer is 30 rpm, the mixing pressure is 4.5 MPa, the cooling water temperature is 30°C, and the rotor temperature is 30°C.