Preparation method of modified rapeseed oil softening agent

By alcoholylation, oxidation and sulfite treatment of rapeseed oil, the epoxy structure and sulfonic acid groups are formed, which solves the problem of poor permeability of leather softening agents, and achieves effective softening and environmentally friendly results of leather cultural relics .

CN118996023AActive Publication Date: 2024-11-22ZHEJIANG SCI-TECH UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410935598.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-22
Estimated Expiration
2044-07-12

AI Technical Summary

Technical Problem

The existing leather softening agent is difficult to penetrate fully into the leather cultural relics, resulting in unsatisfactory softening effect, and the traditional softening agent is not environmentally friendly.

Method used

Modified rapeseed oil is used as leather softener, and the molecular weight and viscosity are reduced through alcoholylation reaction, followed by oxidation and sulfite treatment, and epoxy structure and sulfonic acid groups are introduced to improve permeability and water solubility.

Benefits of technology

It significantly improves the softness and emulsion stability of leather cultural relics, enhances the permeability and emulsion stability of the softening agent, and is environmentally friendly and has good self-emulsification properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004941229950000071
    Figure BDA0004941229950000071
  • Figure BDA0004941229950000081
    Figure BDA0004941229950000081
  • Figure HDA0004941229960000011
    Figure HDA0004941229960000011
Patent Text Reader

Abstract

The invention relates to the field of cultural relic protection, and discloses a preparation method of a modified rapeseed oil leather softening agent. The rapeseed oil is used as a main raw material of the leather softening agent, and is subjected to alcoholysis reaction with methanol to introduce excessive hydroxyl, so that the molecular weight and viscosity of the rapeseed oil can be reduced (the softening agent can permeate into leather favorably), and the rapeseed oil can be used as an intermediate to carry out other reactions; on the basis, hydrogen peroxide is continuously utilized to oxidize carbon-carbon double bonds in the rapeseed oil to form an epoxy structure, so that the antioxidant stability of the rapeseed oil can be improved; furthermore, sulfitation modification is carried out on the water-soluble polycarboxylate superplasticizer, sulfonic acid groups are introduced to molecules, the water solubility of the water-soluble polycarboxylate superplasticizer can be remarkably enhanced, and the water-soluble polycarboxylate superplasticizer has good self-emulsifying performance. Therefore, the finally obtained leather softening agent has excellent permeability and emulsion stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of cultural relics protection, and in particular to a method for preparing a modified rapeseed oil leather softening agent. Background Art

[0002] Leather products are closely related to human civilization and social development. Their applications are not limited to clothing and other daily necessities, but also include applications in various aspects such as transportation, military, culture and art. A large number of leather cultural relics unearthed or handed down in my country are of great value in verifying Chinese civilization. Since the main component of leather, protein, is easily degraded by adverse factors such as microorganisms, light, heat, acid, and alkali, leather cultural relics are difficult to preserve, so the number of unearthed leather cultural relics is relatively small. Compared with other types of organic cultural relics, leather cultural relics are more difficult to protect because of their diverse materials, complex tanning process, and unknown deterioration mechanism.

[0003] Existing leather artifacts have problems such as dryness, discoloration, hardening, decay, and mildew, which endanger the long-term preservation of leather artifacts. Softening agents are a type of preparation that can lubricate leather fiber tissue, giving it a certain degree of toughness, softness, mechanical strength, and ductility. In the softening process of leather artifacts, the softening agent first emulsifies the leather surface through emulsification, then diffuses into the leather, evenly distributes on the fiber surface of the leather, continuously penetrates inward, and finally fills the collagen fibers and their gaps, thereby making the leather artifacts soft.

[0004] However, since leather artifacts are in a state of long-term water loss and hardening, the collagen fibers inside them are more tightly bonded than ordinary leather products, resulting in the leather softening agents currently used being difficult to fully penetrate into the interior of the leather artifacts, and the softening effect is generally less than ideal. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides a preparation method of a modified rapeseed oil leather softening agent. The present invention uses rapeseed oil as the main raw material of the leather softening agent, firstly conducts alcoholysis reaction with methanol to introduce excess hydroxyl groups, which can not only reduce the molecular weight and viscosity of rapeseed oil (which is conducive to the softening agent penetrating into the leather), but also allow it to undergo other reactions as an intermediate; on this basis, continue to use hydrogen peroxide to oxidize the carbon-carbon double bonds in the rapeseed oil to form an epoxy structure, which can improve the antioxidant stability of rapeseed oil; further, sulfiting modification is performed to introduce sulfonic acid groups on the molecule, which can significantly enhance its water solubility and have good self-emulsification properties. Therefore, the leather softening agent finally obtained has excellent permeability and emulsion stability.

[0006] The specific technical scheme of the present invention is: a method for preparing a modified rapeseed oil leather softening agent, comprising the following steps:

[0007] 1) Evenly mix rapeseed oil and methanol, add sodium methoxide as a catalyst; stir and reflux at 60-65° C., and carry out alcoholysis reaction under an inert atmosphere; the mass ratio of methanol to rapeseed oil is 3-4:1.

[0008] 2) After the reaction is completed, the excess methanol is recovered by distillation under reduced pressure, the reaction product is allowed to stand, and the upper oil layer is separated to obtain alcoholysed rapeseed oil.

[0009] 3) mixing alcoholyzed rapeseed oil, acetic acid and a catalyst, stirring and heating to 50-56° C., and dripping hydrogen peroxide (30%) into the system for reaction. The amount of acetic acid used is 7-11% of the mass of the alcoholyzed rapeseed oil; the amount of hydrogen peroxide (25-35wt%) used is 40-45% of the mass of the alcoholyzed rapeseed oil.

[0010] 4) Add alkali to the reaction system for neutralization, let it stand, and remove the water layer after the layers are separated.

[0011] 5) The product obtained in step 4) is washed with water, allowed to stand, and the water layer is removed to obtain epoxidized modified rapeseed oil.

[0012] 6) heating the epoxidized modified rapeseed oil to 50-60° C. and slowly adding a sodium bisulfite aqueous solution dropwise to react; the amount of the sodium bisulfite used is 20-30% of the mass of the epoxidized modified rapeseed oil;

[0013] 7) Add 1-3 wt% of sodium dodecyl sulfate to the system in step 6), raise the temperature to 80-90° C. and stir evenly to obtain a modified rapeseed oil leather softening agent.

[0014] Rapeseed oil is an eco-friendly material and is easily degradable. The present invention finds that using it as the main raw material of a leather softening agent can provide good filling properties for leather. However, the shortcoming of rapeseed oil is that there are fewer functional groups in its molecular structure that can be firmly combined with collagen fibers. For this reason, the present invention introduces hydroxyl groups into the rapeseed oil molecule and reduces the molecular weight of rapeseed oil through chemical modification, and then performs epoxidation modification on it. The epoxidized oil is a three-membered ring compound with high reaction activity, and is sulfited with sodium bisulfite to introduce a sodium sulfonate group so that it has good self-emulsification ability, thereby solving the above problems.

[0015] In step 1), the present invention modifies rapeseed oil by introducing excessive hydroxyl groups, which can not only reduce the molecular weight and viscosity of rapeseed oil (favorable for the softening agent to penetrate into the leather), but also allow it to undergo epoxidation reaction as an intermediate.

[0016] The present invention finds that in the alcoholysis reaction, the ratio of methanol to rapeseed oil is critical. If the alcohol-to-oil ratio is too low, the alcoholysis degree is low and the purpose of modification cannot be achieved; if the alcohol-to-oil ratio is too high, the separation of glycerol will be affected and the conversion rate cannot be improved. Finally, the present invention finds that the alcohol-to-oil ratio has the best effect when it is in the range of 3-4:1.

[0017] In step 3), the carbon-carbon double bonds in the rapeseed oil are oxidized by hydrogen peroxide to form an epoxy structure. The epoxidation reaction can reduce the iodine value of the rapeseed oil and improve the antioxidant stability of the rapeseed oil.

[0018] In step 6), the epoxidized rapeseed oil has an epoxy structure, and then sodium bisulfite aqueous solution is added to sulfite the epoxy structure, and a hydrophilic sodium sulfonate group (-SO3Na) is introduced on the carbon chain, which can significantly enhance its water solubility and have good self-emulsification properties. Therefore, the modified rapeseed oil finally obtained has better permeability and emulsion stability than the sulfated softening agent.

[0019] The present invention finds that the amount of sodium bisulfite used in the sulfiting reaction is critical. If the amount of sodium bisulfite used is too low, the product emulsification is poor and the emulsion stability is poor. If the amount of sodium bisulfite used is too high, there is a lot of residual sulfite, which directly affects the softening effect when it exceeds a certain content. Finally, the present invention finds that the sodium bisulfite accounts for 20-30% of the mass of the epoxidized modified rapeseed oil, which has the best effect.

[0020] Preferably, in step 1), the rapeseed oil is pre-dried and deacidified.

[0021] Preferably, in step 1), the alcoholysis reaction time is 2-3 hours.

[0022] Preferably, in step 3), the catalyst is a strongly acidic cation exchange resin.

[0023] Preferably, in step 3), the amount of the catalyst used is 4.5-5.0% by mass of the rapeseed oil.

[0024] Preferably, in step 3), the reaction time is 20-40 min.

[0025] Preferably, in step 4), the base is a KOH solution.

[0026] Preferably, in step 6), the reaction time is 15-25 min.

[0027] Preferably, in step 7), the stirring time is 2-3 hours.

[0028] Compared with the prior art, the beneficial effects of the present invention are:

[0029] (1) The present invention uses rapeseed oil as the main raw material of the leather softening agent, firstly carries out alcoholysis reaction with methanol to introduce excessive hydroxyl groups, which can not only reduce the molecular weight and viscosity of rapeseed oil (helping the softening agent to penetrate into the leather interior), but also allow it to undergo other reactions as an intermediate; on this basis, continue to utilize hydrogen peroxide to oxidize the carbon-carbon double bonds in the rapeseed oil to form an epoxy structure, which can improve the antioxidant stability of rapeseed oil; further, sulfiting modification is carried out to introduce sulfonic acid groups on the molecule, which can significantly enhance its water solubility and have good self-emulsification properties. Therefore, the final leather softening agent has excellent permeability and emulsion stability.

[0030] (2) The leather softening agent prepared by the method of the present invention is used to soften leather cultural relics, which can significantly improve the softness of the leather cultural relics. In addition, the leather softening agent is environmentally friendly and harmless to the leather cultural relics. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 It is the color difference between aged leather and after softening.

[0032] Figure 2 It is the tensile strength and elongation at break of aged leather before and after softening. DETAILED DESCRIPTION

[0033] The present invention will be further described below in conjunction with the embodiments.

[0034] Example 1

[0035] Step 1): Slowly add methanol and rapeseed oil (pre-dried and deacidified) in a mass ratio of 3:1 into a 250mL three-necked flask and stir for 20 minutes. Add 0.5wt% sodium methoxide of rapeseed oil into the three-necked flask. Raise the temperature to 60°C and react at a constant temperature for 3 hours. After the reaction is completed, filter the product to obtain alcoholysed rapeseed oil.

[0036] Step 2): Add alcoholyzed rapeseed oil, 9% acetic acid by mass of alcoholyzed rapeseed oil and 4.5% strong acid cation exchange resin (cationic resin (732)) to a 250 mL three-necked flask, heat to 50° C., and react for 30 minutes. Slowly add 40% hydrogen peroxide (30%) of alcoholyzed rapeseed oil through a dropping funnel, and the addition is completed within 30 minutes. Add 4.0% KOH solution to adjust the pH to neutral. After the reaction is completed, the product is separated and washed with water several times, and the water layer is removed to obtain epoxidized modified rapeseed oil.

[0037] Step 3): The epoxidized modified rapeseed oil is transferred into a 250 mL three-necked flask with a stirring and reflux device, and an aqueous sodium bisulfite solution is slowly added at 55° C. to react for 20 minutes, wherein the amount of sodium bisulfite is 20% of the mass of the epoxidized modified rapeseed oil, and then 2% of sodium dodecyl sulfate is added, the temperature is raised to 80° C., and stirred for 2.5 hours to obtain a modified rapeseed oil leather softening agent.

[0038] Example 2

[0039] Step 1): Slowly add methanol and rapeseed oil (pre-dried and deacidified) in a mass ratio of 4:1 into a 250mL three-necked flask and stir for 20 minutes. Add 0.5wt% sodium methoxide of rapeseed oil into the three-necked flask. Raise the temperature to 60°C and react at a constant temperature for 3 hours. After the reaction is completed, filter the product to obtain alcoholysed rapeseed oil.

[0040] Step 2): Add alcoholyzed rapeseed oil, 9% acetic acid by mass of alcoholyzed rapeseed oil and 4.5% strong acid cation exchange resin (cationic resin (732)) to a 250 mL three-necked flask, heat to 50° C., and react for 30 minutes. Slowly add 40% hydrogen peroxide (30%) of alcoholyzed rapeseed oil through a dropping funnel, and the addition is completed within 30 minutes. Add 4.0% KOH solution to adjust the pH to neutral. After the reaction is completed, the product is separated and washed with water several times, and the water layer is removed to obtain epoxidized modified rapeseed oil.

[0041] Step 3): The epoxidized modified rapeseed oil is transferred into a 250 mL three-necked flask with a stirring and reflux device, and an aqueous sodium bisulfite solution is slowly added at 55° C. to react for 20 min, wherein the amount of sodium bisulfite is 30% of the mass of the epoxidized modified rapeseed oil, and then 2% of sodium dodecyl sulfate is added, the temperature is raised to 80° C., and stirred for 2.5 h to obtain a modified rapeseed oil leather softening agent.

[0042] Comparative Example 1 (with Example 1 as a reference, the difference is that the alcohol-to-oil ratio in step 1) is 2:1)

[0043] Step 1): Slowly add methanol and rapeseed oil (pre-dried and deacidified) in a mass ratio of 2:1 into a 250mL three-necked flask and stir for 20 minutes. Add 0.5wt% sodium methoxide of rapeseed oil into the three-necked flask. Raise the temperature to 60°C and react at a constant temperature for 3 hours. After the reaction is completed, filter the product to obtain alcoholysed rapeseed oil.

[0044] Step 2): Add alcoholyzed rapeseed oil, 9% acetic acid by mass of alcoholyzed rapeseed oil and 4.5% strong acid cation exchange resin (cationic resin (732)) to a 250 mL three-necked flask, heat to 50° C., and react for 30 minutes. Slowly add 40% hydrogen peroxide (30%) of alcoholyzed rapeseed oil through a dropping funnel, and the addition is completed within 30 minutes. Add 4.0% KOH solution to adjust the pH to neutral. After the reaction is completed, the product is separated and washed with water several times, and the water layer is removed to obtain epoxidized modified rapeseed oil.

[0045] Step 3): The epoxidized modified rapeseed oil is transferred into a 250 mL three-necked flask with a stirring and reflux device, and an aqueous sodium bisulfite solution is slowly added at 55° C. to react for 20 minutes, wherein the amount of sodium bisulfite is 20% of the mass of the epoxidized modified rapeseed oil, and then 2% of sodium dodecyl sulfate is added, the temperature is raised to 80° C., and stirred for 2.5 hours to obtain a modified rapeseed oil leather softening agent.

[0046] Comparative Example 2 (with Example 1 as a reference, the difference is that the alcohol-to-oil ratio in step 1) is 5:1)

[0047] Step 1): Slowly add methanol and rapeseed oil (pre-dried and deacidified) in a mass ratio of 5:1 into a 250mL three-necked flask and stir for 20 minutes. Add 0.5wt% sodium methoxide of rapeseed oil into the three-necked flask. Raise the temperature to 60°C and react at a constant temperature for 3 hours. After the reaction is completed, filter the product to obtain alcoholysed rapeseed oil.

[0048] Step 2): Add alcoholyzed rapeseed oil, 9% acetic acid by mass of alcoholyzed rapeseed oil and 4.5% strong acid cation exchange resin (cationic resin (732)) to a 250 mL three-necked flask, heat to 50° C., and react for 30 minutes. Slowly add 40% hydrogen peroxide (30%) of alcoholyzed rapeseed oil through a dropping funnel, and the addition is completed within 30 minutes. Add 4.0% KOH solution to adjust the pH to neutral. After the reaction is completed, the product is separated and washed with water several times, and the water layer is removed to obtain epoxidized modified rapeseed oil.

[0049] Step 3): The epoxidized modified rapeseed oil is transferred into a 250 mL three-necked flask with a stirring and reflux device, and an aqueous sodium bisulfite solution is slowly added at 55° C. to react for 20 minutes, wherein the amount of sodium bisulfite is 20% of the mass of the epoxidized modified rapeseed oil, and then 2% of sodium dodecyl sulfate is added, the temperature is raised to 80° C., and stirred for 2.5 hours to obtain a modified rapeseed oil leather softening agent.

[0050] Comparative Example 3 (with Example 1 as a reference, the difference is that the amount of sodium bisulfite used in step 3) is 15% of the mass of the epoxidized modified rapeseed oil)

[0051] Step 1): Slowly add methanol and rapeseed oil (pre-dried and deacidified) in a mass ratio of 3:1 into a 250mL three-necked flask and stir for 20 minutes. Add 0.5wt% sodium methoxide of rapeseed oil into the three-necked flask. Raise the temperature to 60°C and react at a constant temperature for 3 hours. After the reaction is completed, filter the product to obtain alcoholysed rapeseed oil.

[0052] Step 2): Add alcoholyzed rapeseed oil, 9% acetic acid by mass of alcoholyzed rapeseed oil and 4.5% strong acid cation exchange resin (cationic resin (732)) to a 250 mL three-necked flask, heat to 50° C., and react for 30 minutes. Slowly add 40% hydrogen peroxide (30%) of alcoholyzed rapeseed oil through a dropping funnel, and the addition is completed within 30 minutes. Add 4.0% KOH solution to adjust the pH to neutral. After the reaction is completed, the product is separated and washed with water several times, and the water layer is removed to obtain epoxidized modified rapeseed oil.

[0053] Step 3): The epoxidized modified rapeseed oil is transferred into a 250 mL three-necked flask with a stirring and reflux device, and an aqueous sodium bisulfite solution is slowly added at 55° C. to react for 20 min, wherein the amount of sodium bisulfite is 15% of the mass of the epoxidized modified rapeseed oil, and then 2% of sodium dodecyl sulfate is added, the temperature is raised to 80° C., and stirred for 2.5 h to obtain a modified rapeseed oil leather softening agent.

[0054] Comparative Example 4 (with Example 1 as a reference, the difference is that the amount of sodium bisulfite used in step 3) is 35% of the mass of the epoxidized modified rapeseed oil)

[0055] Step 1): Slowly add methanol and rapeseed oil (pre-dried and deacidified) in a mass ratio of 3:1 into a 250mL three-necked flask and stir for 20 minutes. Add 0.5wt% sodium methoxide of rapeseed oil into the three-necked flask. Raise the temperature to 60°C and react at a constant temperature for 3 hours. After the reaction is completed, filter the product to obtain alcoholysed rapeseed oil.

[0056] Step 2): Add alcoholyzed rapeseed oil, 9% acetic acid by mass of alcoholyzed rapeseed oil and 4.5% strong acid cation exchange resin (cationic resin (732)) to a 250 mL three-necked flask, heat to 50° C., and react for 30 minutes. Slowly add 40% hydrogen peroxide (30%) of alcoholyzed rapeseed oil through a dropping funnel, and the addition is completed within 30 minutes. Add 4.0% KOH solution to adjust the pH to neutral. After the reaction is completed, the product is separated and washed with water several times, and the water layer is removed to obtain epoxidized modified rapeseed oil.

[0057] Step 3): The epoxidized modified rapeseed oil is transferred into a 250 mL three-necked flask with a stirring and reflux device, and an aqueous sodium bisulfite solution is slowly added at 55° C. to react for 20 min, wherein the amount of sodium bisulfite is 35% of the mass of the epoxidized modified rapeseed oil, and then 2% of sodium dodecyl sulfate is added, the temperature is raised to 80° C., and stirred for 2.5 h to obtain a modified rapeseed oil leather softening agent.

[0058] Application Example 1:

[0059] (1) Preparation of aged leather samples: Cut 10 cm × 10 cm samples from vegetable tanned cowhide. The samples are taken from similar locations on both sides of the back of the same cowhide to ensure similar performance. The samples are placed in a forced air drying oven at 150°C for 8 h.

[0060] (2) Cut a sample of about 3 cm × 3 cm from the aged leather sample, then weigh the aged leather sample, measure its size and softness, and record the data.

[0061] (3) Softening of aged samples: Spray a small amount of 2A solution (anhydrous ethanol and deionized water in a ratio of 1:1) on the surface of the aged leather sample, let it stand for 20 minutes, and use a soft brush to apply the softening agent to the leather surface in small amounts several times until the surface is covered with a thin layer of softening agent. Wait for the softening agent to penetrate completely, wipe off the remaining softening agent on the surface and weigh it. Repeat the softening operation 5 times until saturation is reached, and measure the mass, size, and softness of the sample.

[0062] The performance of the softened leather samples was tested:

[0063] (1) Emulsion stability test:

[0064] ①1:9 dilution stability: Take 90mL of hot distilled water at about 55℃ and put it into a 100mL stoppered measuring cylinder, add 10mL of the sample, plug the measuring cylinder tightly, turn it upside down for 1min, shake it well, and then let it stand at 28℃ for 24h.

[0065] ②Stability of 1 mol / L ammonia solution: Take 80 mL of hot distilled water at about 55°C in a 100 mL stoppered measuring cylinder, add 10 mL of the sample, shake well, then add 10 mL of ammonia solution, plug the measuring cylinder stopper, turn it upside down for 1 min, shake well, and then let it stand at 25-30°C for 24 h.

[0066] ③Stability of 1 mol / L hydrochloric acid solution: Take 80 mL of hot distilled water at about 55°C in a 100 mL stoppered measuring cylinder, add 10 mL of the sample, shake well, then add 10 mL of HCI solution, plug the measuring cylinder stopper, turn up and down for 1 min, shake well, and then let it stand at 28°C for 24 h.

[0067] (2) Color difference test: Using unaged leather as the standard sample, use a colorimeter to select 3 different points on the same softened aged leather sample for color difference test and calculate the average value.

[0068] (3) Softness: Use a softness tester to test the softness of three points on the surface of the same leather sample and take the average value.

[0069] (4) Tensile test: The tensile stress and elongation at break of leather samples were tested using an electronic universal material testing machine in accordance with the national standard QB / T 2710-2018.

[0070] Performance comparison

[0071] Table 1 Performance of different softening agents

[0072]

[0073] Considering the emulsion stability, acid resistance, alkali resistance, color and storage stability, the performance of softener 1# is the most ideal. The amount of sodium bisulfite directly affects the emulsification of the softener. If the amount added is small, the emulsification is poor and the emulsion stability is not good; if the amount added is large, there will be more residual sulfite in the softener, which will affect the emulsification stability of the softener.

[0074] from Figure 1 It can be seen that after the aged leather was treated with the softening agent, the leather surface regained a certain gloss, and the color of the leather sample became fuller, so there was a certain color difference compared to before softening. Among them, the color difference of softening agent 1# changed the most compared to before softening, indicating that the gloss of the aged leather was stronger after softening. The alcohol-oil molar ratio in softening agent 1# was 3:1, the degree of alcoholysis reaction was the largest, the molecular weight and viscosity of rapeseed oil were reduced, the softening agent easily penetrated into the leather and combined with the fiber, and the softening effect was good.

[0075] Table 2 Changes in softness of aged leather after softening

[0076]

[0077] As shown in Table 2, Figure 2 As shown, the softness and mechanical properties of the aged leather samples are improved after softening, the softening agent emulsion penetrates into the collagen fibers, and part of the softening agent components are filled between the collagen fibers. The softening agent has better acid resistance and electrolyte resistance after sulfiting, which makes the leather softer and fuller after softening. When the dosage of sodium bisulfite is 20%, the degree of sulfiting is high, which improves the uniformity of the softening agent dispersion in the leather, improves the softening effect, and improves the mechanical properties of the leather. It shows that the softening agent in the present invention has good permeability and filling properties for leather cultural relics. Rapeseed oil is an eco-friendly material, easy to degrade, and harmless to cultural relics.

[0078] The raw materials and equipment used in the present invention, unless otherwise specified, are all commonly used raw materials and equipment in the art; the methods used in the present invention, unless otherwise specified, are all conventional methods in the art.

[0079] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing a modified rapeseed oil leather softening agent, Features The following steps are involved: 1) Evenly mix rapeseed oil and methanol, add sodium methoxide as a catalyst; stir and reflux at 60-65° C., and perform alcoholysis reaction under an inert atmosphere; the mass ratio of methanol to rapeseed oil is 3-4:1; 2) distilling under reduced pressure after the reaction is completed to recover excess methanol, leaving the reaction product to stand, separating the upper oil layer, and obtaining alcoholysed rapeseed oil; 3) mixing alcoholyzed rapeseed oil, acetic acid and a catalyst, stirring and heating to 50-56° C., and dropping hydrogen peroxide (30%) into the system to react; The acetic acid is used in an amount of 7-11% of the mass of the alcoholyzed rapeseed oil; the concentration of the hydrogen peroxide is 25-35wt%, and the amount used is 40-45% of the mass of the alcoholyzed rapeseed oil; 4) adding alkali to the reaction system for neutralization, allowing it to stand, and removing the water layer after stratification; 5) washing the product obtained in step 4) with water, allowing it to stand, and removing the water layer to obtain epoxidized modified rapeseed oil; 6) heating the epoxidized modified rapeseed oil to 50-60° C., adding a sodium bisulfite aqueous solution dropwise to react; The amount of sodium bisulfite used is 20-30% of the mass of the epoxidized modified rapeseed oil; 7) Add 1-3 wt% of sodium dodecyl sulfonate to the system in step 6), heat to 80-90° C. and stir evenly to obtain a modified rapeseed oil leather softening agent.

2. The preparation method according to claim 1, Features: In step 1), the rapeseed oil is pre-dried and deacidified.

3. The preparation method according to claim 1, Features: In step 1), the alcoholysis reaction time is 2-3 hours.

4. The preparation method according to claim 1, Features: In step 3), the catalyst is a strongly acidic cation exchange resin.

5. The preparation method according to claim 4, Features: In step 3), the amount of the catalyst used is 4.5-5.0% of the mass of the rapeseed oil.

6. The preparation method according to claim 1, Features: In step 3), the reaction time is 20-40 min.

7. The preparation method according to claim 1, Features: In step 4), the base is KOH solution.

8. The preparation method according to claim 1, Features: In step 6), the reaction time is 15-25 min.

9. The preparation method according to claim 1, Features: In step 7), the stirring time is 2-3 hours.

Citation Information

Patent Citations

  • Preparation method of modified rapeseed oil fat-liquoring complex agent

    CN102618673A

  • Preparation method of dry and hard leather cultural-relic softener

    CN103589813A

  • Synthetic fatting agent as well as preparation method and application thereof

    CN112679712A

  • Fat liquoring agent for leather

    EP0564980A1