Steel strand with excellent anti-fatigue performance and production method thereof
By optimizing the alloy element ratio and controlled rolling and cooling technology, the fatigue resistance of prestressed steel strands is improved, and the fatigue performance problem of insufficient fatigue under high stress amplitude in the existing technology is solved, and high strength and high fatigue at 2000MPa level are achieved. performance reduces production costs.
Patent Information
- Application Number
- CN202411429673.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-14
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-10-14
AI Technical Summary
The fatigue performance of existing prestressed steel strands under high stress amplitude is insufficient and cannot meet the high strength and fatigue requirements of the 2000MPa level.
By optimizing the alloy element ratio and controlled rolling and cooling technology, adjusting the chemical composition and production process of the strip, improving the plasticity and tensile strength of the strip, meeting the fatigue requirements under high stress amplitude, including in the production of steel strands, Use C: 0.80%-0.85%, Si: 0.40%-0.55%, Mn: 0.65%-0.75%, Cr: 0.16%-0.22%, V: 0.01-0.04%, Cr+V≤0.25%, Al: 0.01 -0.03%, P≤0.015%, S≤0.015%, and specific heating, rolling, cooling and stabilization treatments are carried out.
The 2,000MPa grade steel strand has achieved 2 million fatigue tests under 360MPa stress amplitude without fracture, which has improved the market competitiveness of fatigue resistance and production costs.
Smart Images

Figure CN118996262A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a steel strand with excellent fatigue resistance and a production method thereof, belonging to the technical field of metallurgy. Background Art
[0002] Prestressed steel strands have the characteristics of high tensile strength, low relaxation value and good fatigue resistance. They are widely used in the construction of roads, bridges, airports, water conservancy dams and other projects. With the rapid development of my country's infrastructure, the annual demand for prestressed steel strands has maintained an increase of more than 10%, and its strength requirements have gradually developed from 1860MPa to 2000MPa and above. At present, the 2000MPa level is the most widely used. On the other hand, with the improvement of the requirements for the bearing capacity and safety of prestressed steel strands, the requirements for their fatigue performance are also gradually increasing. In some structural systems such as prestressed cables, the load of steel strands has the characteristics of large fluctuations, which puts higher requirements on the stress amplitude during fatigue testing. At present, the requirements for fatigue stress amplitude of prestressed cables have been increased to more than 300MPa. The wire rods produced with conventional components and processes cannot meet the use requirements of high-strength and high-fatigue performance steel strands.
[0003] In the prior art, for example, the application with publication number CN 1778981A discloses a microalloying method for producing wire rods for steel strands. By adding a certain amount of Cr and V to 82B, the diameter of pearlite pellets is reduced, the phase transition point is lowered, the pearlite interlamellar spacing suitable for drawing is obtained, the tensile strength of the wire rod is increased, and the drawing performance of the wire rod is improved. The 13mm wire rod produced by the method can be used to draw 2000MPa steel strands. However, this application uses Cr combined with V microalloying to improve the strength of the wire rod. The V content added to its composition is above 0.065%, and the alloy cost is relatively high. In addition, the process window is narrow, and the Cr content needs to be adjusted according to the monthly changes to adapt to the cooling rate in different months, which is complicated to operate. In addition, the wire rod produced by the method can be used to draw 2000MPa steel strands, but it cannot meet the fatigue requirements under high stress amplitudes.
[0004] Therefore, in order to solve the above problems, it is urgent to provide a steel strand that can meet the high stress amplitude fatigue requirements of 2000MPa grade steel strands. Summary of the invention
[0005] The present invention provides a steel strand with excellent fatigue resistance and a production method thereof, which fully utilizes existing equipment conditions, optimizes the alloy element ratio, and adjusts the additional controlled rolling and controlled cooling process to improve the plasticity of the wire rod under the existing production level, thereby improving the tolerance to surface defects to meet the high stress amplitude fatigue requirements of 2000MPa grade steel strands.
[0006] The technical solution adopted by the present invention to solve the technical problem is: A steel strand with excellent fatigue resistance, the wire rod used to make the steel strand includes the following chemical elements by mass fraction: C: 0.80%-0.85%, Si: 0.40%-0.55%, Mn: 0.65%-0.75%, Cr: 0.16%-0.22%, V: 0.01-0.04%, Cr+V≤0.25%, Al: 0.01-0.03%, P≤0.015%, S≤0.015%, and the rest is iron and unavoidable impurities; According to the production method of the steel strand with excellent fatigue resistance, the method specifically comprises the following steps: Step S1: heating in a heating furnace, setting the preheating section temperature of the heating furnace according to the surface temperature of the billet when entering the furnace, the preheating section temperature range is 910-1000°C, and the heating section temperature is set to 1070-1110°C, the soaking section temperature is set to 1120-1160°C, the heating time is set to 60-70min, the air-fuel ratio is ≤0.65, and the rolling start temperature is 1020-1040°C; Step S2: multi-stand continuous rolling, the heated raw materials are preliminarily rolled by rough rolling equipment, and finishing rolling is performed on the basis of rough rolling, during which the inlet temperature is set to 920-950°C and the outlet temperature is ≤1000°C; Step S3: After finishing rolling, cooling is performed by controlling the flow rates of different water tanks, and the spinning temperature is set to 890-900°C; Step S4: Stelmore phase change cooling, 10 fans are set on the Stelmore air cooling line, numbered from 1 to 10, fans numbered 1 to 6 are turned on 100%, fans numbered 7 to 8 are turned on 50%, and fans numbered 9 to 10 are turned on 100%; Step S5: After Stelmor cooling, the wire rods are rolled up to form wire rods; Step S6: Select wire rods that meet quality requirements for drawing, and twist the steel wires to form steel strands; Step S7: Stabilizing and coiling the steel strands, setting the stabilization temperature to 450-460° C., and the treatment time to 80-100 seconds; Further, in step S1, when the surface temperature of the blank is less than 300°C when entering the furnace, the temperature of the preheating section of the heating furnace is set to 960-1000°C; when the surface temperature of the blank is greater than or equal to 300°C when entering the furnace, the temperature of the preheating section of the heating furnace is set to 910-950°C; Furthermore, in step S2, during the finish rolling, the maximum temperature of the entire finish rolling process is maintained at ≤ 1000°C; Further, in step S3, after finishing rolling, cooling is performed by flow control of 5 water tanks, which are numbered from 1 to 5, and only the water tanks numbered 1, 3 and 5 are opened, and the water tanks numbered 2 and 4 are closed, and the flow rate of the water tank numbered 1 is set to 1500-1800 L / min, the flow rate of the water tank numbered 3 is set to 1100-1300 L / min, and the flow rate of the water tank numbered 5 is set to 550-650 L / min; Furthermore, in step S4, the air volume of the fan configured on the Stelmor air cooling line is 280,000 m 3 ; During the operation of the fan, the phase change temperature is maintained at 580-620℃; Further, in step S6, the wire rod is drawn 9 times to form a steel wire with a diameter of 5.06-5.20 mm; Furthermore, the wire rod produced by steps S1-S5 of the production method has a tensile strength of ≥1250MPa, a surface reduction rate of ≥40%, a troostite ratio of ≥90%, a grain size finer than grade 8.5, no complete decarburization, and a semi-decarburized layer depth of ≤0.1mm; Furthermore, the steel strand produced by steps S6-S7 in the production method did not break after 2 million tests when a cyclic load of 360 MPa was applied in an axial fatigue test.
[0007] Through the above technical solution, compared with the prior art, the present invention has the following beneficial effects: 1. The steel strand with excellent fatigue resistance provided by the present invention makes full use of the influence of various elements on the strength and plasticity of steel, obtains wire rods with excellent organization and mechanical properties through the associated design of alloy elements, and has low production cost, which can improve market competitiveness; 2. The production method of the steel strand with excellent anti-fatigue performance provided by the present invention, under the premise of the design scheme of the chemical composition of the wire rod used to make the steel strand, uses the existing equipment level to design the controlled rolling and controlled cooling process, so as to ensure the strengthening effect of the alloy elements and the acquisition of excellent structure, and fully considers the release of the internal stress of the material in the process design during the wire rod production and steel strand stabilization treatment. The obtained steel strand is subjected to a 360MPa stress amplitude fatigue performance test, which can meet the requirement of 2 million times without breaking. BRIEF DESCRIPTION OF THE DRAWINGS
[0008] The present invention is further described below in conjunction with the accompanying drawings and embodiments.
[0009] Figure 1 The present invention is a flowchart of a method for producing a steel strand with excellent fatigue resistance. DETAILED DESCRIPTION
[0010] The present invention is now described in further detail in conjunction with the accompanying drawings. In the description of this application, the specific dimensions used in the embodiments are only for illustrating the technical solution and do not limit the protection scope of the present invention.
[0011] As described in the background technology, the wire rods produced in the prior art can be used to draw 2000MPa steel strands, but cannot meet the fatigue requirements under high stress amplitudes in fatigue tests. Therefore, it is necessary to produce a steel strand that can meet the drawing requirements of 2000MPa steel strands and meet relevant fatigue requirements tests.
[0012] In order to achieve the above requirements, it is necessary to start from the fatigue test itself. Here we will explain in detail what the fatigue test for steel strands is. The fatigue test of steel strands is tensile fatigue. Before the fatigue test, it is necessary to apply a certain tension to both ends of the steel strands, and then conduct the fatigue test under a given stress amplitude. If there is a high axial tensile stress on the surface of the steel strand, when the fatigue test is carried out, after the axial tensile stress is applied to it, the tensile stress on the surface of the steel wire will be superimposed, and failure will occur when the tensile stress on the surface of the steel wire exceeds its yield strength.
[0013] Therefore, the fatigue stress amplitude of steel strand can be increased by improving the residual stress distribution state of steel wire and reducing the surface residual stress of steel wire. Obviously, there are two factors that affect the fatigue resistance of steel wire, namely residual stress and redistribution and diffusion of interstitial atoms.
[0014] The biggest innovation of this application is that it makes full use of existing equipment conditions, optimizes the ratio of alloy elements, and combines the adjustment of the entire steel strand production process to improve the plasticity of the wire rod under the existing production level, thereby meeting both the drawing conditions and the fatigue resistance requirements.
[0015] First of all, regarding the design of each chemical element, the wire rod used to make steel strand includes the following chemical elements in mass fraction: C: 0.80%-0.85%, Si: 0.40%-0.55%, Mn: 0.65%-0.75%, Cr: 0.16%-0.22%, V: 0.01-0.04%, Cr+V≤0.25%, Al: 0.01-0.03%, P≤0.015%, S≤0.015%, and the rest are iron and unavoidable impurities.
[0016] The above-mentioned chemical element components are set according to their respective characteristics. For example, C is the most economical strengthening element in steel materials. Increasing the C content can increase the initial strength of the wire rod; however, an increase in the C content will make the toughness of the wire rod poor and make segregation difficult to control. Therefore, in this application, the C content is controlled to 0.80-0.85%.
[0017] Mn can improve the hardenability of steel, thereby improving the strength and hardness of steel. Mn can also combine with the harmful element S to reduce the hot brittleness of steel. However, a high Mn content will lead to core segregation and grain coarsening. Therefore, in this application, the Mn content is controlled to 0.65-0.75%.
[0018] Cr can effectively improve the hardenability of steel and increase the work hardening rate during cold drawing of steel wire; however, too high a Cr content will reduce the toughness of the steel, and Cr has a greater tendency to segregate, which can easily lead to the formation of core martensite. Therefore, in this application, the Cr content is controlled to 0.16-0.22%.
[0019] V can form fine vanadium carbide or carbonitride compounds with elements such as C and N in steel, and exists in cementite to play a strengthening role, which can make up for the insufficient strength caused by Stelmor controlled cooling; in the cold drawing process, since V strengthens cementite and reduces the deformation coordination of pearlite, it will aggravate the fragmentation of cementite and affect the mechanical properties of steel wire. Therefore, as a micro-alloying element, the content of V should be controlled at 0.01-0.04%.
[0020] It should also be noted that both Cr and V can significantly reduce the bainite transformation temperature, causing the bainite and pearlite regions to transform and separate, increasing the tendency of bainite formation; therefore, the total amount of Cr and V should be controlled below 0.25%.
[0021] Al is a deoxidizing element that removes free oxygen in steel. It can also refine grains and improve the plasticity of steel. In order to achieve better deoxidation and toughening effects, in this application, the aluminum content is controlled to 0.01-0.03%.
[0022] As for P and S, both are harmful elements and their contents should be as low as possible. Therefore, in this application, the contents of P and S are controlled below 0.015%.
[0023] When designing chemical elements, one of the biggest highlights is the Si element. As a commonly used deoxidizer, Si can be dissolved in ferrite to play a role in solid solution strengthening, which can improve the strength and hardenability of wire rods. The segregation tendency of Si is much lower than that of Mn and Cr, and its cost is low. Therefore, by adding Si, the amount of Mn and Cr added can be reduced. However, with the increase of Si content, the area reduction rate of steel is significantly reduced; therefore, in this application, the Si element content is controlled at 0.40%-0.55%.
[0024] Secondly, the present application also provides a method for producing the steel strand with excellent fatigue resistance. Figure 1 As shown, the specific steps include: Step S1: heating in a heating furnace. The preheating section temperature of the heating furnace is set according to the surface temperature of the blank when entering the furnace. The preheating section temperature range is 910-1000°C. Specifically, when the surface temperature of the blank is <300°C when entering the furnace, the preheating section temperature of the heating furnace is set to 960-1000°C; when the surface temperature of the blank is ≥300°C when entering the furnace, the preheating section temperature of the heating furnace is set to 910-950°C.
[0025] At the same time, the heating section temperature is set to 1070-1110°C, the soaking section temperature is set to 1120-1160°C, the heating time is set to 60-70min, the air-fuel ratio is ≤0.65, and the rolling temperature is set to 1020-1040°C.
[0026] The above setting of parameters in the heating furnace can, on the one hand, control the wire rod without complete decarburization, and the depth of the semi-decarburized layer is ≤0.1mm; on the other hand, it can control the growth of grains, which is conducive to a more uniform distribution of interstitial atoms in the billet, thereby reducing the residual stress caused by uneven organization during the phase change process and eliminating the residual stress generated during the solidification process of the billet. In particular, the setting of the preheating section temperature is determined by the surface temperature of the billet before entering the furnace (the temperature is determined by hot charging or cold charging). If the surface temperature of the billet before entering the furnace is 300℃ or above, the temperature range of the preheating section is reduced by 50℃ relative to room temperature, which can reduce the billet surface heating rate, increase the core-surface temperature difference, increase the speed of the core residual heat transfer to the outside, reduce the residence time of the billet in the high temperature section, and avoid the coarsening of the core grains.
[0027] Step S2: Multi-stand continuous rolling, the heated raw materials are initially rolled by rough rolling equipment, and finishing rolling is performed on the basis of rough rolling. During finishing rolling, the inlet temperature is set to 920-950°C, and the outlet temperature is ≤1000°C. Finer austenite grains can be obtained by low-temperature rolling, thereby improving the plasticity of the wire rod.
[0028] Step S3: After finishing rolling, cooling is performed by flow control of different water tanks. The coordination of opening and closing of the water tanks and the water flow rate not only avoids the sharp drop of the surface temperature of the wire rod, but also facilitates the recovery of the surface temperature and the uniformity of the core and surface temperature. Specifically, cooling is performed by flow control of 5 water tanks, which are numbered from 1 to 5, and only the water tanks numbered 1, 3 and 5 are opened, and the water tanks numbered 2 and 4 are closed. The flow rate of the water tank numbered 1 is set to 1500-1800 L / min, the flow rate of the water tank numbered 3 is set to 1100-1300 L / min, and the flow rate of the water tank numbered 5 is set to 550-650 L / min.
[0029] At the same time, the spinning temperature is set to 890-900℃. After spinning, the cooling rate of the core and surface of the wire rod is close, the cooling is more uniform, and the difference in the core and surface structure is small. The reason for setting the spinning temperature range is that a higher spinning temperature can increase the supercooling of austenite, reduce the phase transformation temperature, and increase the cooling rate before the phase transformation.
[0030] In this step, the opening and closing of the water volume in the water cooling box is controlled under the premise of ensuring the spinning temperature, and rapid cooling and temperature recovery are carried out after rolling to make the temperature of the entire cross-section of the wire rod as uniform as possible, thereby reducing the residual stress inside the wire rod before the phase change, so as to reduce the stress inside the wire rod after rolling; at the same time, it promotes the reduction of the grain size of the wire rod and the diameter of the troostite pellets, so that the wire rod obtained after air cooling has higher plasticity.
[0031] Step S4: Stelmore phase change cooling, the air volume of the fan configured on the Stelmore air cooling line is 280,000 m 3 Therefore, 10 fans are set up and numbered from 1 to 10. The fans numbered 1 to 6 are turned on 100%, and the cooling rate before the phase transformation can reach 14-15℃ / s. Increasing the cooling rate before the phase transformation can make the wire rod quickly cool to below the formation temperature of network cementite to avoid the formation of network cementite; fans numbered 7-8 are turned on 50%, and fans numbered 9-10 are turned on 100% to avoid the formation of bainite structure due to too low temperature in the early stage of phase transformation and the high temperature recovery due to the release of latent heat of phase transformation in the latent heat of phase transformation in the latent heat of phase transformation. The phase transformation temperature is maintained at 580-620℃, and the proportion of troostite can be increased to more than 90%.
[0032] Step S5: After Stelmor cooling, the wire rod is rolled up to form a wire rod; at this time, the wire rod produced through steps S1-S5 has a tensile strength ≥1250MPa, a surface reduction rate ≥40%, a sorbite ratio ≥90%, a grain size finer than grade 8.5, no full decarburization, and a semi-decarburized layer depth ≤0.1mm. All of the above indicators of the obtained wire rod fully meet the existing technical requirements for the production of Φ15.2mm specification and 2000MPa strength level steel strand.
[0033] Next is the production process of steel strands, step S6: select wire rods that meet the quality requirements and draw them 9 times to form steel wires with a diameter of 5.06-5.20 mm, and then twist the steel wires to form steel strands.
[0034] Step S7: Stabilize the steel strands and roll them up, and pack them after the rolling is completed. During the stabilization treatment, the stabilization treatment temperature is set to 450-460° C., and the treatment time lasts for 80-100 seconds.
[0035] Step S7 is a more prominent innovation in the steel strand production process. Here it needs to be explained in conjunction with the setting of the Si element content in the chemical composition design. In order to improve the strength of conventional products, the stabilization treatment temperature will be lower, but the lower stabilization temperature is not conducive to the release of steel wire stress. This application reduces the speed of cementite spheroidization during the stabilization treatment of the steel strand and reduces the strength loss by reasonably increasing the Si element content in the steel strand (the Si element content is controlled at 0.40%-0.55%), so that the heating temperature can be increased to 450-460°C during the stabilization treatment of the steel strand. Increasing the heating temperature will promote the thermal motion of atoms, accelerate the diffusion of interstitial atoms, and make the residual stress more fully released, thereby improving the fatigue resistance of the ultra-high strength steel strand.
[0036] In addition, after testing, when the stabilization treatment is carried out at 450-460℃, as the heating time increases, the axial residual stress on the surface of the steel wire tends to increase first and then gradually decrease; but if the heating time is too long, the dislocation density will decrease and the relaxation performance will deteriorate. Therefore, the stabilization treatment time of 80-100s can keep the residual stress on the surface of the steel wire at a low level, so that the atoms have enough time to diffuse and redistribute, and ensure the stability of the relaxation performance.
[0037] Finally, the steel strand produced by steps S6-S7 of the production method did not break after 2 million tests when a 360 MPa cyclic load was applied in an axial fatigue test, thereby greatly improving the service life.
[0038] It will be understood by those skilled in the art that, unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as generally understood by those skilled in the art to which this application belongs. It should also be understood that terms such as those defined in common dictionaries should be understood to have meanings consistent with the meanings in the context of the prior art, and will not be interpreted with idealized or overly formal meanings unless defined as herein.
[0039] The meaning of "and / or" described in this application means that the situations where each exists alone or both exist at the same time are included.
[0040] The term “connection” as used in this application may mean a direct connection between components or an indirect connection between components via other components.
[0041] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.
Claims
1. A steel strand with excellent fatigue resistance, Features: The wire rod used to make steel strand includes the following chemical elements in mass fraction: C: 0.80%-0.85%, Si: 0.40%-0.55%, Mn: 0.65%-0.75%, Cr: 0.16%-0.22%, V: 0.01-0.04%, Cr+V≤0.25%, Al: 0.01-0.03%, P≤0.015%, S≤0.015%, and the rest are iron and unavoidable impurities.
2. The method for producing the steel strand with excellent fatigue resistance according to claim 1, Features: The specific steps include: Step S1: heating in a heating furnace, setting the preheating section temperature of the heating furnace according to the surface temperature of the billet when entering the furnace, the preheating section temperature range is 910-1000°C, and the heating section temperature is set to 1070-1110°C, the soaking section temperature is set to 1120-1160°C, the heating time is set to 60-70min, the air-fuel ratio is ≤0.65, and the rolling start temperature is 1020-1040°C; Step S2: multi-stand continuous rolling, the heated raw materials are preliminarily rolled by rough rolling equipment, and finishing rolling is performed on the basis of rough rolling, during which the inlet temperature is set to 920-950°C and the outlet temperature is ≤1000°C; Step S3: After finishing rolling, cooling is performed by controlling the flow rates of different water tanks, and the spinning temperature is set to 890-900°C; Step S4: Stelmore phase change cooling, 10 fans are set on the Stelmore air cooling line, numbered from 1 to 10, fans numbered 1 to 6 are turned on 100%, fans numbered 7 to 8 are turned on 50%, and fans numbered 9 to 10 are turned on 100%; Step S5: After Stelmor cooling, the wire rods are rolled up to form wire rods; Step S6: Select wire rods that meet quality requirements for drawing, and twist the steel wires to form steel strands; Step S7: Stabilize the steel strands and coil them up, set the stabilization temperature to 450-460°C, and last for 80-100 seconds.
3. The method for producing the steel strand with excellent fatigue resistance according to claim 2, Features: In step S1, when the surface temperature of the blank is less than 300°C when entering the furnace, the temperature of the preheating section of the heating furnace is set to 960-1000°C; when the surface temperature of the blank is greater than or equal to 300°C when entering the furnace, the temperature of the preheating section of the heating furnace is set to 910-950°C.
4. The method for producing a steel strand having excellent fatigue resistance according to claim 2, Features: In step S2, during the finish rolling, the maximum temperature of the entire finish rolling process is maintained at ≤ 1000°C.
5. The method for producing the steel strand with excellent fatigue resistance according to claim 2, Features: In step S3, after finishing rolling, cooling is performed through flow control of 5 water tanks, which are numbered from 1 to 5, and only water tanks numbered 1, 3 and 5 are opened, and water tanks numbered 2 and 4 are closed. The flow rate of water tank numbered 1 is set to 1500-1800 L / min, the flow rate of water tank numbered 3 is set to 1100-1300 L / min, and the flow rate of water tank numbered 5 is set to 550-650 L / min.
6. The method for producing the steel strand with excellent fatigue resistance according to claim 2, Features: In step S4, the air volume of the fan configured on the Stelmor air cooling line is 280,000 m 3 ; During the operation of the fan, the phase change temperature is maintained at 580-620℃.
7. The method for producing the steel strand with excellent fatigue resistance according to claim 2, Features: In step S6, the wire rod is drawn 9 times to form a steel wire with a diameter of 5.06-5.20 mm.
8. The method for producing the steel strand with excellent fatigue resistance according to claim 2, Features: The wire rod produced by steps S1-S5 in the production method has a tensile strength of ≥1250MPa, an area reduction rate of ≥40%, a troostite ratio of ≥90%, a grain size finer than grade 8.5, no complete decarburization, and a semi-decarburization layer depth of ≤0.1mm.
9. The method for producing the steel strand with excellent fatigue resistance according to claim 2, Features: The steel strand produced by steps S6-S7 in the production method did not break after 2 million tests when a 360 MPa cyclic load was applied in an axial fatigue test.
Citation Information
Patent Citations
2400-MPa-strength prestressed steel strand and production process thereof
CN111321352A
Hot-rolled wire rod for annealing-free gas shielded welding wire and preparation method of hot-rolled wire rod
CN114875303A
Wire rod and preparation method and application thereof
CN116716555A
Wire rod for ballastless track plate steel wire of high-speed railway and production method of wire rod
CN116815052A
Production process of steel DL75 hot-rolled wire rod for cable steel strand
CN118326233A