Preparation method and application of double-perovskite water electrolysis hydrogen production and oxygen evolution catalyst
The double perovskite catalyst prepared by the sol-gel method and high-temperature thermal spraying technology solves the problems of high cost and insufficient stability of noble metal-based electrocatalysts, and achieves high performance and long life of the electrode.
Patent Information
- Application Number
- CN202411058485.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-22
AI Technical Summary
Existing precious metal-based electrocatalysts are expensive and lack stability, have poor electrode coating adhesion, and exhibit unstable performance and short lifespan in oxygen-rich environments.
A double perovskite catalyst was prepared by sol-gel method. Combined with high-temperature thermal spraying technology, nickel powder and aluminum powder were mixed with the double perovskite catalyst, sintered on the surface of a metal substrate, and then alkali washed. The resulting double perovskite electrode has good chemical stability and high adhesion.
It improves the conductivity and specific surface area of the electrode, enhances the activity and robustness of the electrode, and makes the catalyst stable and longer-lasting in oxygen-rich environments.
Smart Images

Figure CN118996502A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of water electrolysis hydrogen production catalysts, and in particular to a preparation method and application of a double perovskite water electrolysis hydrogen production oxygen evolution catalyst. Background Art
[0002] Current industrial oxygen evolution electrocatalysts mainly rely on precious metal-based electrocatalysts, such as iridium oxide and ruthenium oxide. However, the storage capacity of precious metals is low, resulting in relatively high costs. In addition, the stability of current precious metal-based electrocatalysts still cannot meet the current development needs. Therefore, it is urgent to synthesize efficient and stable oxygen evolution electrocatalysts to reduce the amount of precious metals used, thereby reducing costs and promoting large-scale commercial use.
[0003] Perovskite oxide is a multi-metal oxide with a general structural formula of ABO. 3 , where A is an alkaline earth metal element, such as Ba and Sr, an alkali metal element, such as Li and Na, or a rare earth metal element, such as La and Pr, and B is a transition metal element, such as Mn, Co, Fe, and Ni. Perovskite oxides have rich structural tunability, and the A and B ions can be replaced or partially replaced by a variety of metal ions with different radii and valences. The transformation of A and B cations can change the crystal and electronic structure characteristics of perovskite oxides, thereby improving their catalytic performance. Therefore, they are often used as catalysts for the oxygen evolution reaction in OER, i.e., hydrogen production by electrolysis of water.
[0004] Existing experimental data have proven that transition metal iron, cobalt, and nickel-based perovskites have excellent oxygen evolution reaction activity. Among the many oxygen evolution electrocatalysts, perovskite-based oxygen evolution electrocatalysts have good application prospects. Perovskite materials have good high-temperature stability and acid and alkali corrosion resistance. Therefore, the prepared perovskite-based oxygen evolution electrocatalyst has a longer life. In an oxygen-rich environment, it will not be denatured due to oxidation, and at the same time, the stability will not be affected by acid and alkali corrosion. In addition, it has more flexible operability when preparing electrodes. It can be prepared by using mild coating methods, such as ultrasonic spraying, scraping and brushing, or by using violent coating methods, such as plasma spraying, supersonic flame spraying and other thermal spraying technologies.
[0005] At present, the preparation methods of electrodes mostly adopt in-situ growth, electrodeposition, ultrasonic spraying, scraping and brushing to apply the catalyst to the surface of the substrate. However, the electrode coating of these preparation methods is not strong, has limited adhesion, and is more dependent on binders. However, most binders are easily detached due to acid and alkali corrosion, and easily lead to decreased conductivity. In addition, the current catalysts mostly use LDH, i.e. layered double hydroxides, iron-nickel oxides and sulfides. However, in nutrient-rich and electrochemical environments, the catalysts are prone to surface reconstruction, lattice oxygen evolution, dissolution, and redeposition, resulting in unstable catalyst performance and shortened life. Summary of the invention
[0006] Based on the technical problems existing in the background technology, the present invention proposes a preparation method and application of a double perovskite water electrolysis hydrogen production and oxygen evolution catalyst.
[0007] The present invention provides a method for preparing a double perovskite water electrolysis hydrogen evolution catalyst, comprising the following steps:
[0008] S1, dissolving cerium salt, strontium salt, copper salt and nickel salt in deionized water to obtain a first mixed solution;
[0009] S2, adding ethanol to the first mixed solution, stirring and ultrasonically treating the solution to obtain a cerium strontium copper nickel precursor;
[0010] S3, adding polyvinyl polypyrrolidone to the cerium strontium copper nickel precursor, stirring until dissolved, to obtain a second mixed solution;
[0011] S4, sequentially adding polyacrylic acid and propylene oxide to the second mixed solution, and stirring to obtain a gel;
[0012] S5, allowing the gel to stand and age for a preset time;
[0013] S6, immersed in ethanol;
[0014] S7, pouring out the ethanol and adding deionized water for washing;
[0015] S8, filtering to remove liquid and placing in an air oven for drying;
[0016] S9, placing in a preset muffle furnace for primary calcination and secondary calcination;
[0017] S10, cooling to obtain double perovskite catalyst powder.
[0018] Furthermore, the step of obtaining the double perovskite catalyst after cooling further comprises:
[0019] The chemical formula of the double perovskite catalyst is: Ce 1-xSr x Cu 1-y Ni y O 3 , wherein x=0-0.5, y=0-0.5, x, y are element amounts respectively, 1-x is the element amount of Ce, x is the element amount of Sr, 1-y is the element amount of Cu, and y is the element amount of Ni.
[0020] Furthermore, the filtering to remove the liquid and placing in an air oven for drying step also includes:
[0021] The set temperature of the air oven is 60° C. and the drying time is 6 h.
[0022] Furthermore, the step of placing the mixture in a preset muffle furnace for primary calcination and secondary calcination further includes:
[0023] The first calcination temperature is 150°C-300°C, and the calcination time is 1h-4h;
[0024] The second calcination temperature is 600° C.-1200° C., and the calcination time is 4 h-10 h.
[0025] The present invention provides an application of a double perovskite water electrolysis hydrogen production and oxygen evolution catalyst, wherein the double perovskite catalyst is used in the preparation of a double perovskite electrode.
[0026] Furthermore, the double perovskite electrode is prepared according to the following steps:
[0027] Step 1, weighing the double perovskite catalyst, nickel powder and aluminum powder, mixing them and adding them into a preset ball mill for ball milling until a preset powder particle size is reached to obtain powder;
[0028] Step 2, loading the powder into a preset thermal spraying device;
[0029] Step 3, fixing a preset metal substrate on a workbench, and using the thermal spraying equipment to perform reciprocating linear motion on the metal substrate at a preset spraying distance;
[0030] Step 4: cooling and soaking the metal substrate in 1 mol / L alkali solution;
[0031] Step five, washing with deionized water and drying in an oven to obtain a double perovskite electrode.
[0032] Furthermore, before the step of weighing the double perovskite catalyst, nickel powder and aluminum powder, mixing them and adding them into a preset ball mill for ball milling until a preset powder particle size is reached to obtain the powder, the step further includes:
[0033] The metal substrate is sequentially immersed in HCl, anhydrous ethanol and deionized water, and ultrasonically cleaned; wherein the single cleaning time is 10 minutes; wherein the metal substrate is one of foamed nickel, foamed iron, foamed copper, nickel felt and titanium felt;
[0034] The metal substrate is dried.
[0035] Furthermore, the step of weighing the double perovskite catalyst, nickel powder and aluminum powder, mixing and adding them into a preset ball mill for ball milling until a preset powder particle size is reached also includes:
[0036] The weight percentage of the double perovskite catalyst is 75%-95%;
[0037] The weight percentage of the nickel powder is 2.5%-15%;
[0038] The weight percentage of the aluminum powder is 2.5%-10%.
[0039] Furthermore, the cooling and the step of placing the metal substrate in a 1 mol / L alkali solution for immersion further comprises:
[0040] The soaking time is 10-30 minutes.
[0041] Furthermore, after the step of loading the powder into a preset thermal spraying device, the process further includes:
[0042] Turning on the preheating switch of the thermal spraying equipment until the preset preheating time is reached; wherein the thermal spraying equipment is one of plasma spraying and supersonic flame spraying;
[0043] Turn on the powder feeder in the thermal spraying equipment and adjust the powder feeding gas flow rate; wherein the powder feeding flow rate is 15-20g / min.
[0044] The present invention has the following beneficial effects:
[0045] The present invention mixes strontium salt and nickel salt, and adopts sol-gel method to prepare double perovskite catalyst, and the prepared double perovskite catalyst has higher hydrogen evolution performance in electrolysis of water to produce hydrogen. According to the high temperature resistant characteristics of perovskite, the present invention adopts high temperature thermal spraying technology, adds nickel powder, aluminum powder and double perovskite catalyst to mix, sinters the double perovskite catalyst on the surface of metal substrate, and performs alkali washing, which not only increases the conductivity of electrode, but also increases the specific surface area and activity of electrode, and the prepared double perovskite electrode has large adhesion and high firmness. In addition, the prepared double perovskite catalyst is a perovskite-type material, has good chemical stability, and even in oxygen-rich environment and electrochemical environment, structural reconstruction will not occur, performance is relatively stable, and life is longer. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Figure 1 The process flow chart of the preparation method of a double perovskite water electrolysis hydrogen evolution catalyst proposed by the present invention;
[0047] Figure 2 The linear sweep voltammograms of Examples 1 and 2 of the present invention are shown;
[0048] Figure 3 Example 2 of the present invention and FeCoNi-LDH oxygen evolution catalyst at a constant current of 800 mA / cm 2 The potential-time curve at . DETAILED DESCRIPTION
[0049] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0050] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0051] See attached Figure 1 , a method for preparing a double perovskite water electrolysis hydrogen evolution catalyst, which comprises the following steps:
[0052] S1, dissolving cerium salt, strontium salt, copper salt and nickel salt in deionized water to obtain a first mixed solution;
[0053] S2, adding ethanol to the first mixed solution, stirring and ultrasonically treating the solution to obtain a cerium strontium copper nickel precursor;
[0054] S3, adding polyvinyl polypyrrolidone to the cerium strontium copper nickel precursor, stirring until dissolved, to obtain a second mixed solution;
[0055] S4, sequentially adding polyacrylic acid and propylene oxide to the second mixed solution, and stirring to obtain a gel;
[0056] S5, allowing the gel to stand and age for a preset time;
[0057] S6, immersed in ethanol;
[0058] S7, pour out the ethanol and add deionized water for washing;
[0059] S8, filtering to remove liquid and placing in an air oven for drying;
[0060] S9, placing in a preset muffle furnace for primary calcination and secondary calcination;
[0061] S10, cooling to obtain double perovskite catalyst powder.
[0062] In the above steps, cerium salt, strontium salt, copper salt and nickel salt are first mixed and dissolved in deionized water to obtain a first mixed solution; then a set amount of ethanol is added to the first mixed solution, and stirring and ultrasonic treatment are performed to obtain a cerium strontium copper nickel precursor, wherein the ultrasonic treatment is to use the characteristics of ultrasonic waves to treat an object; then polyvinyl polypyrrolidone is added to the cerium strontium copper nickel precursor, stirred to dissolve it, then a set amount of polyacrylic acid is slowly added dropwise, and then a set amount of propylene oxide is added dropwise, and stirred to form a gel; then the gel is allowed to stand and age for a preset time. In a specific embodiment, the preset time is 12 hours, that is, the gel is allowed to stand and age for 12 hours. Then, the aged gel is immersed in an ethanol solution, the ethanol is poured out, deionized water is added to wash away the residual ethanol, and then the excess liquid is filtered out; the gel is then placed in an air oven for drying. In a specific embodiment, the temperature of the air oven is set to 60°C, and the drying time is 6 hours; the dried gel is then placed in a muffle furnace for primary and secondary calcination; after cooling, a double perovskite catalyst powder is obtained. The present invention mixes strontium salt and nickel salt, and then uses a sol-gel method to prepare a double perovskite catalyst, which has higher OER performance, wherein OER is a hydrogen evolution reaction in the electrolysis of water to produce hydrogen; and the prepared double perovskite catalyst is a perovskite-type material with a general structural formula of ABO 3 Among them, both the A and B sites have strong doping capabilities and good chemical stability. Even in oxygen-rich and electrochemical environments, structural reconstruction will not occur. The performance is relatively stable and the life is longer.
[0063] In this embodiment, the step of cooling to obtain a double perovskite catalyst further includes:
[0064] The chemical formula of the double perovskite catalyst is: Ce 1-x Sr x Cu 1-y Ni y O 3 , wherein x=0-0.5, y=0-0.5, x, y are element amounts respectively, 1-x is the element amount of Ce, x is the element amount of Sr, 1-y is the element amount of Cu, and y is the element amount of Ni.
[0065] In a specific implementation, the chemical formula of the double perovskite catalyst is: Ce 1-x Sr x Cu 1-y Ni y O 3 , wherein x and y are element amounts. In a specific embodiment, the element amounts can be adjusted; in the present application, x=0-0.5, y=0-0.5, 1-x is the element amount of Ce, x is the element amount of Sr, 1-y is the element amount of Cu, and y is the element amount of Ni.
[0066] In this embodiment, the step of filtering to remove the liquid and placing in an air oven for drying further includes:
[0067] The set temperature of the air oven was 60°C and the drying time was 6 h.
[0068] The step of placing the mixture in a preset muffle furnace for primary calcination and secondary calcination also includes:
[0069] The first calcination temperature is 150°C-300°C, and the calcination time is 1h-4h;
[0070] The second calcination temperature is 600° C.-1200° C., and the calcination time is 4 h-10 h.
[0071] In the specific implementation, after the gel is soaked in ethanol, the ethanol solution is poured out, and deionized water is added to wash away the residual ethanol, and then the liquid is filtered; the prepared gel is placed in an air oven, the temperature is set to 60°C, and dried for 6 hours. The dried gel is placed in a muffle furnace for secondary calcination, wherein the muffle furnace is a box furnace; the temperature of the first calcination is 150°C-300°C, and the calcination time is 1h-4h; then the second calcination is performed, the temperature of the second calcination is 600°C-1200°C, and the calcination time is 4h-10h.
[0072] The present invention provides an application of a double perovskite water electrolysis hydrogen production and oxygen evolution catalyst, which is applied to the preparation of a double perovskite electrode; the double perovskite electrode is prepared according to the following steps:
[0073] Step 1, weighing a double perovskite catalyst, nickel powder and aluminum powder, adding the mixture into a preset ball mill for ball milling until a preset powder particle size is reached to obtain a powder;
[0074] Step 2, loading the powder into a preset thermal spraying device;
[0075] Step 3, fixing a preset metal substrate on a workbench, and performing reciprocating linear motion on the metal substrate at a preset spraying distance through a thermal spraying device;
[0076] Step 4: Cooling and soaking the metal substrate in 1 mol / L alkali solution;
[0077] Step five, washing with deionized water and drying in an oven to obtain a double perovskite electrode.
[0078] In the above steps, first, immerse the metal substrate in HCl, anhydrous ethanol and deionized water in turn for ultrasonic cleaning; each cleaning lasts 10 minutes; wherein, the metal substrate is a solid corrosion-resistant material, which is coated on the surface of a metal or non-metallic substrate to form a tough continuous film to prevent the erosion of the substrate by external corrosive media. Then, the metal substrate is dried for use; the corresponding weight percentages of double perovskite catalyst, nickel powder and aluminum powder are weighed, mixed and added to a preset ball mill for ball milling until a preset powder particle size is reached to obtain a powder; in a specific embodiment, the powder particle size is 100-300 mesh; then, the powder is loaded into a preset powder feeder of a thermal spraying device, and the main power supply, DC power supply, water cooler, argon and hydrogen switches are turned on in turn; wherein, the thermal spraying equipment is one of plasma spraying and supersonic flame spraying; then, the preheating switch in the thermal spraying equipment is turned on for preheating. After the preheating is completed, the powder feeder is turned on, and the powder feeding gas flow rate is adjusted. In the embodiment, the powder feeding flow rate is 15-20g / min; then the pre-treated metal substrate is fixed on the workbench, and the metal substrate is reciprocated linearly at a preset spraying distance by the spray gun of the thermal spraying equipment until the required coating thickness requirement is reached; then it is cooled, and the metal substrate is placed in a 1mol / L alkali solution for immersion; wherein the alkali solution contains more hydroxide, is alkaline, and has strong corrosiveness; in a specific embodiment, the immersion time is 10-30min; finally, it is washed with deionized water to wash away excess alkali solution; then it is placed in an oven for drying to obtain a double perovskite electrode. According to the high temperature resistance characteristics of perovskite, this application adopts high temperature thermal spraying technology, and nickel powder, aluminum powder and double perovskite catalyst are mixed and added, and the double perovskite catalyst is sintered on the surface of the metal substrate, wherein nickel powder can increase the conductivity of the electrode, and aluminum powder can increase the specific surface area and activity of the electrode after alkali washing; so that the prepared coating has the characteristics of high adhesion and high firmness.
[0079] In this embodiment, the double perovskite catalyst, nickel powder and aluminum powder are weighed, mixed and added into a preset ball mill for ball milling until a preset powder particle size is reached. Before the step of obtaining the powder, the step further includes:
[0080] The metal substrate is sequentially immersed in HCl, anhydrous ethanol and deionized water, and ultrasonically cleaned; wherein the single cleaning time is 10 minutes; wherein the metal substrate is one of foamed nickel, foamed iron, foamed copper, nickel felt and titanium felt;
[0081] The metal substrate is dried.
[0082] In the specific implementation, before ball milling, the metal substrate is pretreated: the metal substrate is soaked in HCl, anhydrous ethanol and deionized water in turn, and ultrasonically cleaned for 10 minutes each time, and then dried for use. The metal substrate is one of foamed nickel, foamed iron, foamed copper, nickel felt and titanium felt.
[0083] In this embodiment, the step of weighing a double perovskite catalyst, nickel powder and aluminum powder, mixing and adding the mixture into a preset ball mill for ball milling until a preset powder particle size is reached also includes:
[0084] The weight percentage of the double perovskite catalyst is 75%-95%;
[0085] The weight percentage of nickel powder is 2.5%-15%;
[0086] The weight percentage of the aluminum powder is 2.5%-10%.
[0087] In a specific implementation, after pre-treating the metal substrate, 75%-95% by weight of a double perovskite catalyst, 2.5%-15% by weight of nickel powder and 2.5%-10% by weight of aluminum powder are weighed and mixed, and then added into a ball mill for ball milling until the powder particle size is 100-300 mesh.
[0088] In this embodiment, the step of cooling and placing the metal substrate in a 1 mol / L alkali solution for immersion further includes:
[0089] The soaking time is 10-30 minutes.
[0090] In a specific implementation, after the metal substrate is sprayed, it is cooled, and after cooling, the metal substrate is immersed in 1 mol / L alkaline solution for 10-30 minutes.
[0091] In this embodiment, after the step of loading the powder into the preset thermal spraying equipment, the method further includes:
[0092] Turning on the preheating switch of the thermal spraying equipment until the preset preheating time is reached; wherein the thermal spraying equipment is one of plasma spraying and supersonic flame spraying;
[0093] Turn on the powder feeder in the thermal spraying equipment and adjust the powder feeding gas flow rate; wherein the powder feeding flow rate is 15-20g / min.
[0094] In the specific implementation, the ball-milled powder is loaded into the powder feeder in the thermal spraying equipment, and the switches of the main power supply, DC power supply, water cooler, argon and hydrogen are turned on in sequence, wherein the thermal spraying equipment is one of plasma spraying and supersonic flame spraying. Then the preheating switch is turned on, and after the preheating is completed, the powder feeder is turned on, and the powder feeding gas flow rate is adjusted. In a specific embodiment, the powder feeding gas flow rate is 15-20g / min.
[0095] In summary, in the specific implementation, the preparation of the double perovskite catalyst is as follows: first, cerium salt, strontium salt, copper salt and nickel salt are mixed and dissolved in deionized water to obtain a first mixed solution; then a set amount of ethanol is added to the first mixed solution, and stirred and ultrasonically treated to obtain a cerium strontium copper nickel precursor. The chemical formula of the double perovskite is: Ce 1- x Sr x Cu 1-y Ni y O 3, wherein x=0-0.5, y=0-0.5, x and y represent the amount of elements; then add polyvinyl polypyrrolidone to the cerium strontium copper nickel precursor solution and stir to dissolve it; after stirring and dissolving, slowly add polyacrylic acid, then add propylene oxide, continue to stir until a gel is formed, and then stand and age for 12 hours; soak the aged gel in ethanol, then pour out the ethanol, add deionized water to wash away the residual ethanol, and then continue to filter out the liquid; then put the gel into an air oven and dry it at 60°C for 6 hours, then put the dried gel into a muffle furnace and calcine it at 150°C-300°C for 1-4 hours, and then calcine it at 600°C-1200°C for 4-10 hours; after cooling, a powdery double perovskite catalyst is obtained. Preparation of double perovskite electrode: soak the metal substrate in HCl, anhydrous ethanol and deionized water in turn, and perform ultrasonic cleaning at the same time, each cleaning for 10 minutes; then dry the metal substrate; then weigh 75%-95% of double perovskite catalyst by weight, 2.5%-15% of nickel powder by weight and 2.5%-10% of aluminum powder by weight, mix them, add them to a ball mill after mixing, and mill them until the powder particle size reaches 100-300 mesh; then load the ball-milled powder into the powder feeder of the thermal spraying equipment, turn on the main power supply, DC power supply in turn , water cooler, argon and hydrogen switches, then turn on the preheating switch, turn on the powder feeder after the preheating is completed, adjust the powder feeding gas flow rate, the powder feeding gas flow rate is 15-20g / min; then fix the treated metal substrate on the workbench, use the spray gun of the thermal spraying equipment, and make reciprocating linear motion at the set spraying distance until the coating thickness requirements are met; after cooling, place the sprayed metal substrate in 1mol / L alkali solution and soak it for 10-30min, then wash off the excess alkali solution with deionized water, and finally put it in an oven for drying, thus completing the preparation of the double perovskite electrode.
[0096] See attached Figure 1 , is a method for preparing a double perovskite water electrolysis hydrogen evolution catalyst in one embodiment of the present invention, wherein,
[0097] Example 1
[0098] A method for preparing a double perovskite water electrolysis hydrogen production and oxygen evolution catalyst is prepared according to the following steps:
[0099] S1. dissolving a mixture of cerium salt and copper salt in deionized water;
[0100] S2. Add ethanol, stir and ultrasonicate, mix well, and obtain a cerium copper precursor;
[0101] S3. Add polyvinyl polypyrrolidone and stir to dissolve;
[0102] S4. Slowly add polyacrylic acid and propylene oxide dropwise in sequence, stirring until a gel is formed;
[0103] S5. Aging for 12 hours;
[0104] S6. Soak in ethanol;
[0105] S7. Pour off the ethanol and add deionized water for washing;
[0106] S8. Filter and place in an air oven at 60°C for 6 hours;
[0107] S9. Place in a muffle furnace, set to 250 ° C for 2h, and then set to 900 ° C for 8h;
[0108] S10. Cooling to obtain CeCuO 3 Perovskite catalysts.
[0109] A double perovskite electrode is prepared according to the following steps:
[0110] Step 1: Soak the preset nickel foam substrate in HCl, anhydrous ethanol and deionized water in sequence for ultrasonic cleaning, each cleaning lasting 10 minutes;
[0111] Step 2: drying;
[0112] Step 3: Weigh CeCuO 3 The perovskite catalyst, nickel powder and aluminum powder are mixed and added into a preset ball mill for ball milling until the powder particle size is 100-300 mesh;
[0113] Step 4: Load the powder into the powder feeder of the thermal spraying equipment, and turn on the main power supply, DC power supply, water cooler, argon gas and hydrogen switches in sequence;
[0114] Step 5: Start preheating;
[0115] Step 6, start the powder feeder and adjust the powder feeding gas flow rate, wherein the powder feeding flow rate is 15-20g / min;
[0116] Step 7, fix the metal substrate on the workbench, and make a reciprocating linear motion at a spraying distance through the spray gun of the thermal spraying equipment;
[0117] Step 8: Cooling and soaking the metal substrate in 1 mol / L alkali solution for 10 min to 30 min;
[0118] Step nine, washing with deionized water and drying in an oven to obtain CeCuO 3 Perovskite electrode.
[0119] CeCuO prepared in Example 1 3The perovskite catalyst is a single perovskite, that is, the chemical formula of the double perovskite catalyst is: Ce 1-x Sr x Cu 1-y Ni y O 3 , x=0, y=0.
[0120] Example 2
[0121] A method for preparing a double perovskite water electrolysis hydrogen production and oxygen evolution catalyst is prepared according to the following steps:
[0122] S1. dissolving a mixture of cerium salt, strontium salt, copper salt and nickel salt in deionized water;
[0123] S2. Add ethanol, stir and ultrasonicate, mix well, and obtain a cerium strontium copper nickel precursor;
[0124] S3. Add polyvinyl polypyrrolidone and stir to dissolve;
[0125] S4. Slowly add polyacrylic acid and propylene oxide dropwise in sequence, stirring until a gel is formed;
[0126] S5. Aging for 12 hours;
[0127] S6. Soak in ethanol;
[0128] S7. Pour off the ethanol and add deionized water for washing;
[0129] S8. Filter and place in an air oven at 60°C for 6 hours;
[0130] S9. Place in a muffle furnace, set to 250 ° C for 2h, and then set to 900 ° C for 8h;
[0131] S10. Cool down and obtain the chemical formula Ce 0.8 Sr 0.2 Cu 0.8 Ni 0.2 O 3 Double perovskite catalysts.
[0132] A double perovskite electrode is prepared according to the following steps:
[0133] Step 1: Soak the preset nickel foam substrate in HCl, anhydrous ethanol and deionized water in sequence for ultrasonic cleaning, each cleaning lasting 10 minutes;
[0134] Step 2: drying;
[0135] Step 3: Weigh Ce 0.8 Sr 0.2 Cu 0.8 Ni0.2 O 3 Double perovskite catalyst, nickel powder and aluminum powder are mixed and added into a preset ball mill for ball milling until the powder particle size is 100-300 mesh;
[0136] Step 4: Load the powder into the powder feeder of the thermal spraying equipment, and turn on the main power supply, DC power supply, water cooler, argon gas and hydrogen switches in sequence;
[0137] Step 5: Start preheating;
[0138] Step 6, start the powder feeder and adjust the powder feeding gas flow rate, wherein the powder feeding flow rate is 15-20g / min;
[0139] Step 7, fix the metal substrate on the workbench, and make a reciprocating linear motion at a spraying distance through the spray gun of the thermal spraying equipment;
[0140] Step 8: Cooling and soaking the metal substrate in 1 mol / L alkali solution for 10 min to 30 min;
[0141] Step nine, washing with deionized water and drying in an oven to obtain Ce 0.8 Sr 0.2 Cu 0.8 Ni 0.2 O 3 Double perovskite electrode.
[0142] Example 2 is different from Example 1 in that, in the step of preparing the double perovskite catalyst S1, cerium salt, strontium salt, copper salt and nickel salt are mixed and dissolved in deionized water, ethanol is added, stirred and ultrasonically treated, and mixed evenly to obtain a precursor of cerium strontium copper nickel precursor; in the double perovskite catalyst chemical formula Ce 1-x Sr x Cu 1-y Ni y O 3 , x=0.2, y=0.2.
[0143] The electrochemical performance test was conducted using an electrochemical workstation at room temperature using a membrane electrode electrolytic cell. The cell was a two-electrode system with a 1 mol / L KOH solution as the electrolyte. The electrolyte temperature was 60 °C and the scan rate of the linear sweep voltammogram (LSV) was 10 mV·s -1 , the potential scanning range is 1.0V-2.0V.
[0144] like Figure 2 As shown in the figure, it is the linear sweep voltammogram of Example 1 and Example 2. It can be seen from the figure that the CeCuO obtained in Example 1 3The current density of the perovskite electrode at a cell voltage of 1.8 V is 262 mA cm -2 , Ce obtained in Example 2 0.8 Sr 0.2 Cu 0.8 Ni 0.2 O 3 The current density of the double perovskite electrode at a cell voltage of 1.8 V is 534 mA cm -2 It can be seen that the electrode prepared in Example 2 has higher electrochemical performance, that is, Ce prepared by doping Sr and Ni 0.8 Sr 0.2 Cu 0.8 Ni 0.2 O 3 Double perovskite catalysts have higher OER performance. OER is the oxygen evolution reaction with four electron transfer occurring at the anode in the hydrogen production reaction by water electrolysis.
[0145] Figure 3 Example 2 and FeCoNi-LDH oxygen evolution catalyst at a constant current of 800 mA / cm 2 The potential-time curve of the electrode obtained in Example 2 is 0.25 mV / h in 20 h, and the overpotential decay amplitude of the FeCoNi-LDH electrode is 0.85 mV / h in 20 h. 0.8 Sr 0.2 Cu 0.8 Ni 0.2 O 3 Double perovskite catalysts have higher stability.
[0146] In summary, the Ce prepared in Example 2 0.8 Sr 0.2 Cu 0.8 Ni 0.2 O 3Double perovskite catalyst has high OER performance, and the prepared electrode has higher electrochemical performance. Compared with the prior art, the present application mixes strontium salt and nickel salt, and adopts sol-gel method to prepare double perovskite catalyst, and the prepared double perovskite catalyst has higher hydrogen evolution performance in electrolysis of water to produce hydrogen. According to the high temperature resistant characteristics of perovskite, the present invention adopts high temperature thermal spraying technology, adds nickel powder, aluminum powder and double perovskite catalyst to mix, sinters the double perovskite catalyst on the surface of metal substrate, and performs alkali washing, which not only increases the conductivity of the electrode, but also increases the specific surface area and activity of the electrode, and the prepared double perovskite electrode has large adhesion and high firmness. In addition, the prepared double perovskite catalyst is a perovskite-type material with good chemical stability, and even in oxygen-rich environment and electrochemical environment, structural reconstruction will not occur, the performance is relatively stable, and the service life is longer.
[0147] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for preparing a double perovskite catalyst for hydrogen production and oxygen evolution by water electrolysis, It is characterized in that The following steps are involved: S1, dissolving cerium salt, strontium salt, copper salt and nickel salt in deionized water to obtain a first mixed solution; S2, adding ethanol to the first mixed solution, stirring and ultrasonically treating the solution to obtain a cerium strontium copper nickel precursor; S3, adding polyvinyl polypyrrolidone to the cerium strontium copper nickel precursor, stirring until dissolved, to obtain a second mixed solution; S4, sequentially adding polyacrylic acid and propylene oxide to the second mixed solution, and stirring to obtain a gel; S5, allowing the gel to stand and age for a preset time; S6, immersed in ethanol; S7, pouring out the ethanol and adding deionized water for washing; S8, filtering to remove liquid and placing in an air oven for drying; S9, placing in a preset muffle furnace for primary calcination and secondary calcination; S10, cooling to obtain double perovskite catalyst powder.
2. The method for preparing the double perovskite water electrolysis hydrogen evolution catalyst according to claim 1, It is characterized in that The step of obtaining the double perovskite catalyst after cooling also includes: The chemical formula of the double perovskite catalyst is: Ce 1-x Sr x Cu 1-y Ni y O 3 , wherein x=0-0.5, y=0-0.5, x, y are element amounts respectively, 1-x is the element amount of Ce, x is the element amount of Sr, 1-y is the element amount of Cu, and y is the element amount of Ni.
3. The method for preparing the double perovskite water electrolysis hydrogen production and oxygen evolution catalyst according to claim 1, It is characterized in that The filtering step to remove the liquid and placing the mixture in an air oven for drying also includes: The set temperature of the air oven is 60° C. and the drying time is 6 h.
4. The method for preparing the double perovskite water electrolysis hydrogen production and oxygen evolution catalyst according to claim 1, It is characterized in that The step of placing the mixture in a preset muffle furnace for primary calcination and secondary calcination also includes: The first calcination temperature is 150°C-300°C, and the calcination time is 1h-4h; The second calcination temperature is 600° C.-1200° C., and the calcination time is 4 h-10 h.
5. Application of a double perovskite catalyst for hydrogen production and oxygen evolution in water electrolysis, It is characterized in that The double perovskite catalyst prepared by the method for preparing a double perovskite water electrolysis hydrogen production and oxygen evolution catalyst according to any one of claims 1 to 4 is used in the preparation of a double perovskite electrode.
6. Application of the double perovskite water electrolysis hydrogen production and oxygen evolution catalyst according to claim 5, It is characterized in that The double perovskite electrode is prepared according to the following steps: Step 1, weighing the double perovskite catalyst, nickel powder and aluminum powder, mixing them and adding them into a preset ball mill for ball milling until a preset powder particle size is reached to obtain powder; Step 2, loading the powder into a preset thermal spraying device; Step 3, fixing a preset metal substrate on a workbench, and using the thermal spraying equipment to perform reciprocating linear motion on the metal substrate at a preset spraying distance; Step 4: cooling and soaking the metal substrate in 1 mol / L alkali solution; Step five, washing with deionized water and drying in an oven to obtain a double perovskite electrode.
7. Application of the double perovskite water electrolysis hydrogen production and oxygen evolution catalyst according to claim 6, It is characterized in that The step of weighing the double perovskite catalyst, nickel powder and aluminum powder, mixing and adding them into a preset ball mill for ball milling until a preset powder particle size is reached to obtain a powder further comprises: The metal substrate is sequentially immersed in HCl, anhydrous ethanol and deionized water, and ultrasonically cleaned; wherein the single cleaning time is 10 minutes; wherein the metal substrate is one of foamed nickel, foamed iron, foamed copper, nickel felt and titanium felt; The metal substrate is dried.
8. Application of the double perovskite water electrolysis hydrogen production and oxygen evolution catalyst according to claim 6, It is characterized in that The step of weighing the double perovskite catalyst, nickel powder and aluminum powder, mixing and adding them into a preset ball mill for ball milling until a preset powder particle size is reached, further includes: The weight percentage of the double perovskite catalyst is 75%-95%; The weight percentage of the nickel powder is 2.5%-15%; The weight percentage of the aluminum powder is 2.5%-10%.
9. Application of the double perovskite water electrolysis hydrogen production and oxygen evolution catalyst according to claim 6, It is characterized in that The step of cooling and placing the metal substrate in a 1 mol / L alkali solution for immersion also includes: The soaking time is 10-30 minutes.
10. Use of the double perovskite water electrolysis hydrogen production and oxygen evolution catalyst according to claim 6, It is characterized in that After the step of loading the powder into a preset thermal spraying device, the method further comprises: Turning on the preheating switch of the thermal spraying equipment until the preset preheating time is reached; wherein the thermal spraying equipment is one of plasma spraying and supersonic flame spraying; Turn on the powder feeder in the thermal spraying equipment and adjust the powder feeding gas flow rate; wherein the powder feeding flow rate is 15-20g / min.