Vanadium disulfide / trinickel disulfide composite material as well as preparation method and application thereof

By developing vanadium disulfide/trini nickel disulfide composite as catalysts, the high energy consumption problem of OER in electrocatalytic water decomposition is solved, stable operation and efficient catalysis at low voltages are achieved, and cost-effective solutions are provided.

CN118996509APending Publication Date: 2024-11-22NANCHANG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411233991.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In the prior art, the anode oxygen evolution reaction (OER) with electrocatalytic water decomposition is slow and has high energy consumption, which hinders hydrogen production and has high cost of precious metal catalysts, limiting their widespread application.

Method used

Develop a vanadium disulfide/trininic disulfide composite material (Ni3S2/VS2) to prepare nanorod array material through hydrothermal reaction, as a dual-function catalyst for urea oxidation reaction (UOR) and electrolytic hydrogen evolution reaction (HER). Its multi-active sites and heterogeneous interfaces improve catalytic efficiency.

Benefits of technology

It achieves long-term and stable operation at low battery voltage, reduces energy consumption in hydrogen production, provides cost-effective catalysts, improves catalytic efficiency, and reduces environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996509A_ABST
    Figure CN118996509A_ABST
Patent Text Reader

Abstract

The invention provides a vanadium disulfide / trinickel disulfide composite material as well as a preparation method and application thereof. The method comprises the following steps: pretreating foamed nickel; the preparation method comprises the following steps: adding sodium orthovanadate and thioacetamide into a mixed solution containing deionized water, ammonia water and ethylene glycol, and uniformly stirring to obtain a uniform solution; and mixing the uniform solution with the pretreated foamed nickel to carry out hydrothermal reaction, and cooling to room temperature after the reaction is finished to obtain the vanadium disulfide / trinickel disulfide composite material. The Ni3S2 / VS2 composite material prepared by the invention has abundant active sites, a unique interface and a synergistic effect between Ni3S2 and VS2, so that the catalytic efficiency of a catalyst is effectively improved, and the Ni3S2 / VS2 composite material has a good catalytic effect in a urea oxidation reaction, a water electrolysis hydrogen evolution reaction and a urea auxiliary water electrolysis reaction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of catalyst material preparation, and in particular to a vanadium disulfide / nickel disulfide composite material and a preparation method and application thereof. Background Art

[0002] As a green and renewable energy, hydrogen energy has high energy density and is environmentally friendly, and is regarded as an ideal alternative to traditional fossil fuels. Electrocatalytic water splitting involves the hydrogen evolution reaction (HER) at the cathode and the oxygen evolution reaction (OER) at the anode. However, due to its slow four-proton coupling reaction kinetics, the high overpotential of OER directly hinders the entire water splitting process. Compared with OER, the theoretical potential of urea oxidation reaction (UOR) (0.37Vvs 1.23V) is relatively low. Therefore, replacing OER with UOR can more effectively reduce the energy consumption of hydrogen production, and at the same time can provide a promising method for removing urea from wastewater.

[0003] Noble metal materials are considered as benchmark electrocatalysts for UOR and HER, however, their high cost and limited availability hinder their widespread application; thus, the development of enhanced and cost-effective bifunctional catalysts for UOR and HER is urgently needed. Summary of the invention

[0004] The purpose of the present invention is to provide a vanadium disulfide / nickel disulfide composite material and a preparation method and application thereof, which can provide a new catalyst for UOR, and the vanadium disulfide / nickel disulfide composite material has more active sites and can provide a new catalytic system, which can operate stably for a long time at a low battery voltage in urea-assisted water electrolysis.

[0005] In a first aspect, the present invention provides a method for preparing a vanadium disulfide / nickel disulfide composite material, the method comprising:

[0006] Pre-treating the nickel foam;

[0007] Adding sodium orthovanadate and thioacetamide into a mixed solution containing deionized water, ammonia water and ethylene glycol, stirring evenly to obtain a uniform solution;

[0008] The uniform solution and the pretreated nickel foam are mixed to carry out a hydrothermal reaction, and after the reaction is completed, the mixture is cooled to room temperature to obtain a vanadium disulfide / nickel disulfide composite material.

[0009] Furthermore, the step of adding sodium orthovanadate and thioacetamide to a mixed solution containing deionized water, ammonia water and ethylene glycol and stirring uniformly to obtain a uniform solution comprises:

[0010] adding sodium orthovanadate to a mixed solution containing deionized water, aqueous ammonia and ethylene glycol, and stirring to form a first solution;

[0011] Thioacetamide was added to the first solution, and stirring was continued until the solid was completely dissolved to obtain a uniform solution.

[0012] Furthermore, the step of pretreating the nickel foam comprises:

[0013] The nickel foam was cleaned in 1-5 M hydrochloric acid solution, acetone and deionized water for 8-12 min respectively.

[0014] Furthermore, the volume ratio of deionized water, ammonia water and ethylene glycol is 7-9:0.8-1.2:7-9.

[0015] Furthermore, the amount of sodium orthovanadate added is 0.03-0.18 mmol, and the amount of thioacetamide added is 0.45-0.49 mmol.

[0016] Furthermore, the temperature of the hydrothermal reaction is 140-180° C., and the time of the hydrothermal reaction is 14-18 hours.

[0017] Furthermore, the Ni, S and V elements in the vanadium disulfide / nickel disulfide composite material are evenly distributed.

[0018] Furthermore, the vanadium disulfide / nickel disulfide composite material is a nanorod array material.

[0019] In a second aspect, the present invention provides a vanadium disulfide / nickel disulfide composite material prepared by the above-mentioned preparation method of the vanadium disulfide / nickel disulfide composite material, wherein the sulfur-vanadium ratio in the vanadium disulfide / nickel disulfide composite material is 8:0.5-3.

[0020] In a third aspect, the present invention provides an application of the vanadium disulfide / nickel disulfide composite material as described above in a urea oxidation reaction.

[0021] In a fourth aspect, the present invention provides an application of the vanadium disulfide / nickel disulfide composite material as described above in a hydrogen evolution reaction by electrolysis of water.

[0022] In a fifth aspect, the present invention provides an application of the vanadium disulfide / nickel disulfide composite material as described above in a urea-assisted water electrolysis reaction.

[0023] Compared with the prior art, the present invention has the following advantages:

[0024] (1) The method for preparing the vanadium disulfide / nickel disulfide composite material provided by the present invention has a simple process and does not require the addition of precious metals during the preparation process, which can effectively reduce costs and preparation time.

[0025] (2) The Ni3S2 / VS2 composite material prepared by the present invention has more active sites and forms a heterogeneous interface, which makes the charge transfer more efficient. It can be used as a new electroreaction catalyst and can effectively improve the catalytic efficiency of the catalyst, that is, it has a good catalytic effect in urea oxidation reaction, water electrolysis hydrogen evolution reaction and urea-assisted water electrolysis reaction.

[0026] (3) The Ni3S2 / VS2 composite material provided by the present invention can catalyze urea oxidation reaction and water electrolysis hydrogen evolution reaction in a green and efficient manner under mild reaction conditions with water and urea as electrolytes. The product is green and environmentally friendly, reducing environmental pollution. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a flow chart of a method for preparing a vanadium disulfide / nickel disulfide composite material in one embodiment of the present invention;

[0028] Figure 2 The XRD images of Ni3S2 / VS2 composites, Ni3S2 and NF are compared with the Ni3S2 and VS2 standard cards;

[0029] Figure 3 The SEM images and EDS-mapping element distribution diagrams of Ni3S2 / VS2 composite material and catalyst Ni3S2;

[0030] Figure 4 STM image of Ni3S2 / VS2 composite material;

[0031] Figure 5 XPS images of Ni3S2 / VS2 composite material and catalyst Ni3S2;

[0032] Figure 6 Contact angle test images of Ni3S2 / VS2 composite material, Ni3S2 and NF;

[0033] Figure 7 This is the urea oxidation reaction stability test image of Ni3S2 / VS2 composite material;

[0034] Figure 8 This is the SEM image of the Ni3S2 / VS2 composite material after the urea oxidation reaction stability test;

[0035] Fig. 9 This is the stability test image of the hydrogen evolution reaction of water electrolysis of Ni3S2 / VS2 composite material;

[0036] Fig.10 This is the SEM image of the Ni3S2 / VS2 composite material after the stability test of the electrolytic water hydrogen evolution reaction;

[0037] Fig.11 This is the stability test image of urea-assisted water electrolysis reaction of Ni3S2 / VS2 composite material;

[0038] Fig.12 This is the SEM image of the Ni3S2 / VS2 composite material after the urea-assisted water electrolysis stability reaction test;

[0039] Fig.13 XRD images of Ni3S2 / VS2 composite materials after urea oxidation reaction, water electrolysis hydrogen evolution reaction and urea-assisted water electrolysis reaction stability test;

[0040] Fig.14 The graph shows the electrocatalytic test results of urea oxidation reaction of Ni3S2 / VS2 composite material and catalysts with different S:V molar ratios;

[0041] Fig.15 Electrocatalytic test results of urea oxidation reaction of Ni3S2 / VS2 composite material, catalyst Ni2S3 and NF;

[0042] Fig.16 The electrocatalytic test results of the Ni3S2 / VS2 composite material and catalysts with different S:V molar ratios in the electrolysis of water for hydrogen evolution reaction are shown in the figure;

[0043] Fig.17 The electrocatalytic test results of the Ni3S2 / VS2 composite material, catalyst Ni2S3 and NF for the electrolytic water hydrogen evolution reaction;

[0044] Fig.18 This is the electrocatalytic test results of Ni3S2 / VS2 composite material for urea-assisted water electrolysis reaction.

[0045] The following specific implementation manner will further illustrate the present invention in conjunction with the above-mentioned drawings. DETAILED DESCRIPTION

[0046] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Unless otherwise defined, the technical terms or scientific terms used herein should be understood by people with general skills in the field to which the present invention belongs. "Including" and similar words used in this article mean that the elements or objects appearing before the word include the elements or objects listed after the word and their equivalents, without excluding other elements or objects.

[0047] In the first aspect, please refer to 1, which shows a method for preparing a vanadium disulfide / nickel disulfide composite material in an embodiment of the present invention. The method includes steps S101 to S103, wherein:

[0048] Step S101: pre-treating the nickel foam;

[0049] It should be noted that this step is mainly to clean the nickel foam to remove oil stains, dirt, etc. in the nickel foam. Specifically, in the actual cleaning process, the nickel foam needs to be washed with hydrochloric acid solution, acetone, and deionized water in sequence.

[0050] In some embodiments, the concentration of the hydrochloric acid solution is 1-5M. If the concentration of the hydrochloric acid used for cleaning is too high, it may cause corrosion to the nickel foam itself. If the concentration of the hydrochloric acid used for cleaning is too low, it will affect the cleaning effect. By controlling the concentration of the hydrochloric acid within a suitable range, the hydrochloric acid solution can have a good cleaning effect. By way of example, the concentration of the hydrochloric acid solution can be 1M, 2M, 3M, 4M, 5M, and the like.

[0051] In addition, the cleaning time of the nickel foam in the hydrochloric acid solution, acetone, and deionized water is 8-12 minutes. Exemplarily, the cleaning time of the nickel foam in the hydrochloric acid solution, acetone, and deionized water can be 8 minutes, 10 minutes, 12 minutes, and the like.

[0052] Step S102: adding sodium orthovanadate and thioacetamide to a mixed solution containing deionized water, ammonia water and ethylene glycol, and stirring the mixture to obtain a uniform solution;

[0053] It should also be pointed out that, in some embodiments, sodium orthovanadate and thioacetamide can be added together to the mixed solution containing deionized water, ammonia water and ethylene glycol, or sodium orthovanadate can be added first and then thioacetamide.

[0054] Preferably, sodium orthovanadate is first added to a mixed solution containing deionized water, ammonia water and ethylene glycol, and stirred to form a first solution; thioacetamide is added to the first solution, and stirring is continued until the solid is completely dissolved to obtain a uniform solution.

[0055] In some embodiments, the volume ratio of deionized water, ammonia water and ethylene glycol is 7-9:0.8-1.2:7-9. For example, the volume ratio of deionized water, ammonia water and ethylene glycol can be 7:1:7, 8:1:8, 9:1:9 and the like.

[0056] In some embodiments, the amount of sodium orthovanadate added is 0.03-0.18 mmol, and the amount of thioacetamide added is 0.45-0.49 mmol. If the amount of sodium orthovanadate added is too high, the nanorods of the material will have different morphologies and the catalytic effect will be poor. If the amount of sodium orthovanadate added is too low, the electrocatalytic effect of the material on UOR will be reduced. By controlling the amount of sodium orthovanadate added within a suitable range, the electrocatalytic performance of Ni3S2 / VS2 for UOR, HER, and urea-assisted water electrolysis reactions can achieve the best effect. For example, the amount of sodium orthovanadate added can be 0.03mmol, 0.06mol, 0.12mmol, and 0.18mmol; if the amount of thioacetamide added is too high, the material will become brittle and cannot be used. If the amount of thioacetamide added is too low, the electrocatalytic effect of the material will be reduced. By controlling the amount of thioacetamide added within a suitable range, the Ni3S2 / VS2 material with the best catalytic performance can be obtained. For example, the amount of thioacetamide added can be 0.45mmol, 0.47mol, 0.49mol, and the like.

[0057] Step S103: mixing the uniform solution and the pretreated nickel foam to perform a hydrothermal reaction, and cooling to room temperature after the reaction to obtain a vanadium disulfide / nickel disulfide composite material.

[0058] In some embodiments, the temperature of the hydrothermal reaction is 140-180°C. If the temperature of the hydrothermal reaction is set too high, the material will fall off. If the temperature of the hydrothermal reaction is set too low, the load amount will be reduced. By setting the temperature of the hydrothermal reaction in a suitable range, the load amount on the NF can reach an optimal amount. Exemplarily, the temperature of the hydrothermal reaction can be 140°C, 160°C, 180°C, etc.

[0059] In some embodiments, the reaction time of the hydrothermal reaction is 14h-18h. If the reaction time of the hydrothermal reaction is too short, the loading amount of the NF will be reduced. If the reaction time of the hydrothermal reaction is too long, the physical and chemical properties of the NF will be affected, making it unusable. By controlling the reaction time of the hydrothermal reaction within a suitable range, the material can obtain the best catalytic performance. For example, the reaction time of the hydrothermal reaction can be 14h, 16h, 18h, and so on.

[0060] It should also be noted that after the hydrothermal reaction is completed and cooled to room temperature, the obtained vanadium disulfide / nickel disulfide composite material must be thoroughly washed with deionized water and dried in a vacuum oven at 50-120°C to finally obtain a vanadium disulfide / nickel disulfide composite material product.

[0061] In a second aspect, an embodiment of the present invention further provides a vanadium disulfide / nickel disulfide composite material, and the vanadium disulfide / nickel disulfide composite material is obtained by the above-mentioned preparation method.

[0062] In some embodiments, the sulfur-vanadium ratio is 8:0.5-3. For example, the sulfur-vanadium ratio of the vanadium disulfide / nickel disulfide composite material can be 8:0.5, 8:1, 8:2, 8:3, and the like.

[0063] In addition, it should be pointed out that the vanadium disulfide / nickel disulfide composite material obtained by the above scheme is a nanorod array material.

[0064] In addition, it should be pointed out that the Ni, S, and V elements in the vanadium disulfide / nickel disulfide composite material are evenly distributed.

[0065] In a third aspect, an embodiment of the present invention further provides an application of a vanadium disulfide / nickel disulfide composite material in a urea oxidation reaction (UOR), a water electrolysis hydrogen evolution reaction (HER) and a urea-assisted water electrolysis reaction.

[0066] In some embodiments, the application includes the following steps:

[0067] Electrochemical tests were performed using 1M KOH + 0.3M urea solution as the electrolyte in the urea oxidation reaction (UOR);

[0068] Electrochemical tests were performed using 1M KOH solution as the electrolyte in the hydrogen evolution reaction (HER) during water electrolysis;

[0069] Electrochemical tests were performed using 1M KOH + 0.3M urea as the electrolyte in the urea-assisted water electrolysis reaction;

[0070] In some embodiments, the three electrodes used in the electrochemical test are: a graphite rod as a counter electrode, Hg / HgO as a reference electrode, and a Ni3S2 / VS2 electrode as a working electrode. Each sample is tested at room temperature, and all potentials are iR corrected and the electrode potential is corrected with reference to the reversible hydrogen electrode (RHE) according to the following formula: ERHE = E (Hg / HgO) + 0.098 + 0.059 × pH.

[0071] In some embodiments, the scanning rate in the linear sweep voltammetry (LSV) test of the vanadium disulfide / nickel disulfide composite material is: 5 mV s -1 .

[0072] In some embodiments, the Tafel slope of the vanadium disulfide / nickel disulfide composite material is determined by the following equation: η=b log|j|+a.

[0073] In some embodiments, the electrochemical impedance spectroscopy (EIS) test conditions of the vanadium disulfide / nickel disulfide composite material are: within a frequency range of 100 kHz to 0.01 Hz and with an amplitude of 5 mV.

[0074] In some embodiments, the scanning rates in the electrochemically active surface area (ECSA) test of the vanadium disulfide / nickel disulfide composite material are: 20 mV s -1 , 40mV s -1 , 60mV s -1 , 80mV s -1 and 100mV s -1 .

[0075] Example 1

[0076] Embodiment 1 of the present invention provides a method for preparing a vanadium disulfide / nickel disulfide composite material, comprising the following steps:

[0077] S1. Wash a sheet of nickel foam (size: 2.5 cm×2 cm×0.5 cm) in 3M hydrochloric acid solution, acetone and deionized water for 10 minutes respectively.

[0078] S2. Dissolve 0.06 mmol of sodium orthovanadate in a mixed solution containing 8 ml of deionized water, 1 ml of aqueous ammonia and 8 ml of ethylene glycol, and stir vigorously for 30 minutes to form a first solution.

[0079] S3. Add 0.47 mmol of thioacetamide to the first solution, and continue stirring for 30 minutes until all the solids are dissolved to obtain a uniform solution.

[0080] S4. The obtained homogeneous solution and the cleaned NF (nickel foam) were transferred to an autoclave and hydrothermaled at 160° C. for 16 h. After cooling to room temperature (25° C.), the obtained catalyst was thoroughly washed with deionized water and dried in a vacuum oven at 60° C. for 12 h.

[0081] Example 2

[0082] The technical scheme of this embodiment is basically the same as that of Embodiment 1, except that the dosage of sodium orthovanadate in step S2 is 0.08 mmol, and finally a vanadium disulfide / nickel disulfide composite material with a S:V molar ratio of 8:0.5 is obtained.

[0083] Example 3

[0084] The technical scheme of this embodiment is basically the same as that of Embodiment 1, except that the dosage of sodium orthovanadate in step S2 is 0.08 mmol, and finally a vanadium disulfide / nickel disulfide composite material with a S:V molar ratio of 8:0.5 is obtained.

[0085] Example 4

[0086] The technical scheme of this embodiment is basically the same as that of Embodiment 1, except that the dosage of sodium orthovanadate in step S2 is 0.18 mmol, and finally a vanadium disulfide / nickel disulfide composite material with a S:V molar ratio of 8:3 is obtained.

[0087] Comparative Example 1

[0088] The technical solution of this comparative example is basically the same as that of Example 1, except that sodium orthovanadate is not added in step S2, and a nickel sulfide catalyst is finally obtained.

[0089] Comparative Example 2

[0090] This comparative example provides a method for preparing a nickel sulfide catalyst, which is different from Example 1 in that only the cleaning of the nickel foam in step S1 is completed, and finally a clean pure nickel foam is obtained.

[0091] Comparative Example 3

[0092] The technical scheme of this comparative example is basically the same as that of Example 1, except that the sodium orthovanadate added in step S2 is replaced by ammonium metavanadate and anhydrous sodium molybdate, wherein the amount of ammonium metavanadate added is 0.06 mmol, and the amount of anhydrous sodium molybdate added is 0.02 mmol, to obtain a catalyst.

[0093] Test Example 1

[0094] This test example provides an application of the vanadium disulfide / nickel disulfide composite material prepared in Example 1 in a urea oxidation reaction, specifically including: using 1M KOH + 0.3M urea solution as an electrolyte for electrochemical testing, and the test content is as follows:

[0095] The scan rate in the linear sweep voltammetry (LSV) test is: 5mV s -1 .

[0096] The Tafel slope of the catalyst Ni3S2 / VS2 is determined by the following equation: η=b log|j|+a.

[0097] The electrochemical impedance spectroscopy (EIS) test conditions of the catalyst Ni3S2 / VS2 are: within a frequency range of 100 kHz to 0.01 Hz and with an amplitude of 5 mV.

[0098] The scanning rates in the electrochemically active surface area (ECSA) test of the catalyst Ni3S2 / VS2 are: 20 mVs -1 , 40mV s -1 , 60mV s -1 , 80mV s-1 and 100mV s -1 .

[0099] The stability test of the catalyst Ni3S2 / VS2 was evaluated by a 50 h chronoamperometry and a 2000 cycle CV test.

[0100] Test Example 2

[0101] This test example provides an application of the vanadium disulfide / nickel disulfide composite material prepared in Example 1 in a hydrogen evolution reaction by electrolysis of water, specifically comprising: using 1M KOH solution as an electrolyte for an electrochemical test, and the test content is as follows:

[0102] The scan rate in the linear sweep voltammetry (LSV) test is: 5mV s -1 .

[0103] The Phil slope of the catalyst Ni3S2 / VS2 is determined by the following equation: η=b log|j|+a.

[0104] The electrochemical impedance spectroscopy (EIS) test conditions of the catalyst Ni3S2 / VS2 are: within a frequency range of 100 kHz to 0.01 Hz and with an amplitude of 5 mV.

[0105] The scanning rates in the electrochemically active surface area (ECSA) test of the catalyst Ni3S2 / VS2 are: 20 mVs -1 , 40mV s -1 , 60mV s -1 , 80mV s -1 and 100mV s -1 .

[0106] The stability test of the catalyst Ni3S2 / VS2 was evaluated by a 50 h chronoamperometry and a 2000 cycle CV test.

[0107] Catalyst Ni3S2 / VS2 at -10mA cm -2 The potential of hydrogen evolution by water electrolysis (HER) is 164 mV at a current of .

[0108] Test Example 3

[0109] This test example provides an application of the vanadium disulfide / nickel disulfide composite material prepared in Example 1 in a urea-assisted water electrolysis reaction, specifically including: using 1M KOH+0.3M urea as an electrolyte for electrochemical testing, and the test content is as follows:

[0110] The scan rate in the linear sweep voltammetry (LSV) test is: 5mV s -1 .

[0111] The stability test of the catalyst Ni3S2 / VS2 was evaluated by a 50h chronoamperometry test.

[0112] Catalyst Ni3S2 / VS2 at 10 mA cm -2 The potential of urea-assisted water electrolysis to produce hydrogen is 1.48 V under a current of , and it can be stably tested for 50 hours.

[0113] The test method of Test Example 1 was used to test the products obtained in Examples 2-4 and Comparative Examples 1-3. Please refer to Table 1 below, which shows the test table of the effect of the catalysts prepared in Examples 1-4 and Comparative Examples 1-3 in the urea oxidation reaction:

[0114] Table 1 Effect test table of urea oxidation reaction

[0115]

[0116] The test method of Test Example 2 was used to test the products obtained in Examples 2-4 and Comparative Examples 1-3. Please refer to Table 2 below, which shows the effect test table of the catalysts prepared in Examples 1-4 and Comparative Examples 1-3 in the electrolytic hydrogen evolution reaction (HER):

[0117] Table 2 Effect test table of water electrolysis hydrogen evolution reaction (HER)

[0118]

[0119] The test method of Test Example 3 was used to test the products obtained in Examples 2-4 and Comparative Examples 1-3. Please refer to Table 3 below, which shows the test table of the effect of the catalysts prepared in Examples 1-4 and Comparative Examples 1-3 in urea-assisted water electrolysis reaction:

[0120] Table 3

[0121]

[0122] Results analysis: According to Tables 1 to 3, under the action of the catalyst provided by the present invention, the Ni3S2 / VS2 catalyst provided by the present invention has a conductivity of 100 mA cm -2 Only 1.396V-1.427V is needed for urea oxidation at -10mA cm -2 164-229 mV is required for hydrogen evolution in water electrolysis. As a bifunctional electrocatalyst, urea-assisted Ni3S2 / VS2‖Ni3S2 / VS2 electrolyzer is used at 10 mA cm -2It can operate at a low battery voltage of 1.48V and exhibit long-term stability. The electrocatalytic performance of the material is best when S:V=8:1, and the efficiency of Ni3S2 alone as a catalyst is significantly reduced; this proves that the catalyst provided by the present invention has good catalytic activity and high catalytic efficiency. In addition, according to Tables 1 to 3, it can be seen that whether sodium orthovanadate is not added or sodium orthovanadate is replaced by other vanadium sources, the catalytic effect of the product obtained in the three reactions of urea oxidation reaction and electrolysis of water for hydrogen evolution is poor, indicating that the new composite material obtained under specific conditions according to a specific vanadium source in the present invention has a better catalytic effect.

[0123] Performance Verification

[0124] 1. Characterization of the catalyst Ni3S2 / VS2 prepared by the present invention

[0125] (1) Characterization of crystal structure

[0126] The catalysts prepared in Example 1 and Comparative Example 1 of the present invention were tested by XRD using an X-ray diffractometer. The results are as follows: Figure 2 As shown;

[0127] See also Figure 2 The characteristic diffraction peaks of Ni3S2 and Ni can be clearly observed in the XRD of Ni3S2 / VS2 prepared in Example 1 of the present invention. However, the diffraction peak of VS2 in Ni3S2 / VS2 is not obvious, which may be caused by the low crystallinity or content of VS2 in the material. The diffraction peak of nickel sulfide in Ni3S2 is obvious, proving that the material synthesis is successful.

[0128] (2) Scanning electron microscopy characterization

[0129] The Ni3S2 / VS2 prepared in Example 1 and the Ni3S2 prepared in Comparative Example 1 were characterized by scanning electron microscopy (SEM). Figure 3 As shown;

[0130] See also Figure 3 , Figure 3 (a) is the form of Ni3S2. Figure 3 (b) shows the morphology of Ni3S2 / VS2; Ni3S2 is in the form of nanosheets; Ni3S2 / VS2 is composed of smooth nanoarrays. From the element distribution diagrams (c)-(f), it can be seen that the Ni, S, and V elements of Ni3S2 / VS2 are evenly distributed.

[0131] (3) Transmission electron microscopy characterization

[0132] The Ni3S2 / VS2 prepared in Example 1 was studied using a transmission electron microscope (TEM). Figure 4 As shown;

[0133] See also Figure 4 In (a) and (b), the Ni3S2 / VS2 prepared by the present invention has formed a nanorod structure. The HRTEM image of Ni3S2 / VS2 shows two lattice fringes of different widths, wherein the lattice spacing of 0.18nm corresponds to the (211) plane of Ni3S2 (JCPDS No.02-0772), and the lattice spacing of 0.19nm corresponds to the (104) plane of VS2 (JC PDS No.89-1640). This further confirms the successful preparation of the Ni3S2 / VS2 catalyst, and the catalyst forms a heterogeneous interface.

[0134] (5) XPS characterization

[0135] XPS characterization was used to further study the Ni3S2 / VS2 prepared in Example 1. Figure 5 As shown;

[0136] See also Figure 5 (a)-(c), the XPS spectra of Ni3S2 / VS2 show the signals of Ni, V and S elements, while the XPS spectrum of Ni3S2 shows the signals of Ni and S elements ( Figure 5 (d) and (e)). High-resolution XPS spectra show that the Ni 2p 3 / 2 and Ni 2p 1 / 2 Located at 856.1eV and 870eV respectively. Ni2p 1 / 2 The spectrum has two peaks at 870.1eV and 873.8eV, consistent with the presence of nickel-sulfur species. The two peaks at 879.4eV and 861.1eV correspond to Ni 2+ and Ni 3+ The remaining peaks at 870.0 eV and 852.7 eV are consistent with the characteristic peaks of NF substrate. It is worth noting that compared with Ni3S2, the two strong Ni2p 3 / 2 and 2p 1 / 2 The peaks shift toward higher binding energies. The peaks at 517 eV and 524.5 eV correspond to the V 2p 3 / 2 and V2p 1 / 2 , indicating that V 4+ The core energy level scanning spectrum of S2p has three characteristic peaks. The peaks at 162.5eV and 163.6eV correspond to S 2- S2p of species 3 / 2 and S2p 1 / 2 The characteristic peak near 168.3 eV can be attributed to sulfate ions, indicating that the material is slightly oxidized. Based on the above analysis and discussion, it can be shown that the present invention has successfully prepared Ni3S2 / VS2 nanorod arrays on NF substrates.

[0137] 6) Contact angle characterization

[0138] The contact angle was used to characterize the Ni3S2 / VS prepared in Example 1. 2、 The hydrophobicity and gas repellency of Ni3S2 prepared in Comparative Example 1 and NF prepared in Comparative Example 2 were tested. Figure 6 As shown;

[0139] To further understand the surface properties of Ni3S2 and Ni3S2 / VS2, we performed static droplet (1M KOH alkaline solution) contact angle tests. Figure 6 The “initial” in the figure indicates that the KOH solution droplets begin to approach the bare NF, Ni3S2, and Ni3S2 / VS2 surfaces. Figure 6 (a) It can be clearly seen that when KOH electrolyte droplets are trapped on the bare NF surface, their surface wettability is poor. From 1 second to 15 seconds, the contact angle remains almost constant, always around 139.1°, indicating that the surface of the NF sample is hydrophobic. Surface properties of Ni3S2 catalysts are shown in Figure 2. Figure 6 (b). When the KOH electrolyte droplet is captured by its surface, its contact angle is 129.3°, which proves that the wettability of Ni3S2 catalyst is poor. The interaction between Ni3S2 / VS2 surface and KOH solution droplet is shown in Figure 6 As shown in (c). When the KOH solution drips, the droplet spreads rapidly and the high-speed camera cannot capture the contact angle, which proves that the Ni3S2 / VS2 surface is superhydrophilic. When Ni3S2 / VS2 is constructed on the NF substrate, a large number of polar bonds Ni-S and VS are formed on the surface of the Ni3S2 / VS2 catalyst, and the OH bond in H2O is also a strong polar bond. Therefore, when the KOH solution droplet contacts the surface of the Ni3S2 / VS2 catalyst, a dipole interaction occurs immediately, which changes the surface tension of the KOH solution flow and promotes the rapid diffusion of the KOH solution droplet. Therefore, Ni3S2 / VS2 exhibits superhydrophilicity. Subsequently, the underwater bubble contact angle was measured, as shown in Figure 6 As shown in (d), the contact angles of NF, Ni3S2, and Ni3S2 / VS2 samples were found to be 130.1°, 133.5°, and 149.6°, respectively. This indicates that Ni3S2 / VS2 is superhydrophobic under water. This improved hydrophilicity promotes better contact between the catalyst and the electrolyte solution, aids in gas release, and effectively enhances the electrocatalytic performance.

[0140] 2. Catalyst Cycling Performance Verification for Test Example 1

[0141] The catalyst Ni3S2 / VS2 prepared by the present invention was subjected to 2000 CV cycle tests; Figure 7As shown in (a), the urea oxidation performance of catalyst Ni3S2 / VS2 does not change much before and after the cycle.

[0142] The catalyst Ni3S2 / VS2 prepared by the present invention was tested by chronoamperometry for 50 h; Figure 7 (b) shows that the current drop during the test was not obvious. The SEM image of the catalyst Ni3S2 / VS2 after 50h chronoamperometry test cycle is shown in Figure 8 As shown, the morphology still maintains the nanorod array, proving that the morphology of the catalyst prepared by the present invention is stable.

[0143] 3. Catalyst Cycling Performance Verification for Test Example 2

[0144] The catalyst Ni3S2 / VS2 prepared by the present invention was subjected to 2000 CV cycle tests; Fig. 9 As shown in (a), the performance of catalyst Ni3S2 / VS2 for hydrogen evolution by water electrolysis does not change much before and after the cycle.

[0145] The catalyst Ni3S2 / VS2 prepared by the present invention was tested by chronoamperometry for 50 h; Fig. 9 (b) shows that the current drop during the test was not obvious. The SEM image of the catalyst Ni3S2 / VS2 after 50h chronoamperometry test cycle is shown in Fig.10 As shown, the morphology still maintains the nanorod array, proving that the morphology of the catalyst prepared by the present invention is stable.

[0146] 4. Catalyst Cycling Performance Verification for Test Example 3

[0147] The catalyst Ni3S2 / VS2 prepared by the present invention was tested by chronoamperometry for 50 h; Fig.11 As shown in the figure, the current drop during the test was not obvious. The SEM image of the catalyst Ni3S2 / VS2 after 50h chronoamperometry test cycle is shown in the figure. Fig.12 As shown, the morphology still maintains the nanorod array, proving that the morphology of the catalyst prepared by the present invention is stable.

[0148] Although the embodiments of the present invention are described in detail above, it is obvious to those skilled in the art that various modifications and variations can be made to these embodiments. However, it should be understood that such modifications and variations are within the scope and spirit of the present invention as described in the claims. Moreover, the present invention described herein may have other embodiments and may be implemented or realized in a variety of ways.

Claims

1. A method for preparing a vanadium disulfide / nickel disulfide composite material, characterized in that: The method comprises: Pre-treating the nickel foam; Adding sodium orthovanadate and thioacetamide into a mixed solution containing deionized water, ammonia water and ethylene glycol, stirring evenly to obtain a uniform solution; The uniform solution and the pretreated nickel foam are mixed to carry out a hydrothermal reaction, and after the reaction is completed, the mixture is cooled to room temperature to obtain a vanadium disulfide / nickel disulfide composite material.

2. The method for preparing the vanadium disulfide / nickel disulfide composite material according to claim 1, characterized in that: The step of adding sodium orthovanadate and thioacetamide to a mixed solution containing deionized water, ammonia water and ethylene glycol and stirring uniformly to obtain a uniform solution comprises: adding sodium orthovanadate to a mixed solution containing deionized water, aqueous ammonia and ethylene glycol, and stirring to form a first solution; Thioacetamide was added to the first solution, and stirring was continued until the solid was completely dissolved to obtain a uniform solution.

3. The method for preparing the vanadium disulfide / nickel disulfide composite material according to claim 1, characterized in that: The step of pre-treating the nickel foam comprises: The nickel foam was cleaned in 1-5 M hydrochloric acid solution, acetone and deionized water for 8-12 min respectively.

4. The method for preparing the vanadium disulfide / nickel disulfide composite material according to claim 1, characterized in that: The volume ratio of deionized water, ammonia water and ethylene glycol is 7-9:0.8-1.2:7-9.

5. The method for preparing the vanadium disulfide / nickel disulfide composite material according to any one of claims 1 to 4, characterized in that: The amount of sodium orthovanadate added is 0.03-0.18 mmol, and the amount of thioacetamide added is 0.45-0.49 mmol.

6. The method for preparing the vanadium disulfide / nickel disulfide composite material according to any one of claims 1 to 4, characterized in that: The temperature of the hydrothermal reaction is 140-180°C, and the time of the hydrothermal reaction is 14-18h.

7. A method for preparing a vanadium disulfide / nickel disulfide composite material according to any one of claims 1 to 6, wherein the vanadium disulfide / nickel disulfide composite material is prepared, characterized in that: The sulfur-vanadium ratio in the vanadium disulfide / nickel disulfide composite material is 8:0.5-3.

8. Use of the vanadium disulfide / nickel disulfide composite material as claimed in claim 7 in urea oxidation reaction.

9. Use of the vanadium disulfide / nickel disulfide composite material as claimed in claim 7 in hydrogen evolution reaction by electrolysis of water.

10. Use of the vanadium disulfide / nickel disulfide composite material as claimed in claim 7 in urea-assisted water electrolysis reaction.