Preparation method of chlorine evolution titanium anode with high catalytic activity
By adding ethyl cellulose to the catalytic active layer of the titanium chlorine-eliminated anode and using sandblasting, heat treatment and multiple coating sintering methods, the crack problem on the surface of the anode in the traditional method is solved, and the electrochemical performance is improved. Lifespan increases the effective catalytic area.
Patent Information
- Application Number
- CN202411232252.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-11-22
AI Technical Summary
The surface of the chlorine-eliminated titanium anode prepared by traditional thermal decomposition is prone to cracks, resulting in excessive gas content, reducing the selectivity of chlorine-eliminated, and affecting the anode life and electrocatalytic performance.
Ethyl cellulose is added to the catalytically active layer, and a high catalytically active titanium chloride anode with a large specific surface area and a stable stacking morphology is prepared by sandblasting, heat treatment, acid etching and multiple coating sintering.
The electrochemical performance of the anode is improved, the chlorine overpotential is reduced, the service life of the anode is extended, and the cracks in the coating are slowed down through the template action, increasing the effective catalytic activity area.
Smart Images

Figure CN118996519A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of electrochemical technology, and in particular to a method for preparing a chlorine-evolving titanium anode with high catalytic activity. Background Art
[0002] In recent years, the use of coated titanium electrodes for electrocatalytic chlorine evolution reaction to produce free chlorine has been widely used in seawater electrolysis, brine electrolysis, water treatment, disinfection, etc. As the most commonly used anode material in the chlorine evolution industry, titanium-based metal oxides have good chlorine evolution activity and stability. The traditional method of ruthenium titanium chlorine evolution anode usually adopts thermal decomposition method.
[0003] For example, the invention application with application number CN201711139064.X discloses an anode for chlorine evolution, which is composed of an electrode substrate and a coating coated on the surface of the electrode substrate, wherein the coating is composed of ruthenium oxide, rhodium oxide and titanium oxide, and the loading amount of the ruthenium oxide is 4 to 20 g / m 2 The loading amount of the rhodium oxide is 1 to 10 g / m 2 The mass ratio of the ruthenium oxide to the titanium oxide is 50-70:50-30 in terms of Ru:Ti. The electrode substrate is titanium. The preparation method of the above-mentioned anode for chlorine analysis comprises applying precursor compounds of ruthenium, titanium and rhodium on the surface of the electrode substrate, and sintering to decompose and oxidize the precursor compounds to obtain the anode for chlorine analysis. The sintering temperature is 400-600°C and the time is 5-60 minutes.
[0004] However, the surface microstructure of the electrode prepared by the thermal decomposition method is prone to obvious cracks. When the gas content released during use is too high, it will lead to passivation of the titanium substrate, thereby reducing the chlorine evolution selectivity and affecting the life of the anode.
[0005] The way to optimize the chlorine-evolving titanium anode is to improve its electrocatalytic performance, increase the number of active points on the coating surface, and reduce the chlorine evolution overpotential during the electrocatalytic process. Therefore, the present invention proposes a method for preparing a chlorine-evolving titanium anode with high catalytic activity to overcome the defects of the prior art. Summary of the invention
[0006] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a method for preparing a chlorine-evolving titanium anode with high catalytic activity. By adding ethyl cellulose in the catalytic active layer, the prepared chlorine-evolving titanium anode has a large specific surface area and a stable stacking morphology, providing sufficient electrocatalytic active sites, thereby improving the electrochemical performance of the anode and providing reference for practical applications in the field of chlorine evolution.
[0007] The technical solution adopted by the present invention to solve the technical problem is: a method for preparing a high catalytic activity chlorine-evolving titanium anode, the preparation method comprising the following steps:
[0008] Step 1), pre-treating the surface of the titanium substrate: sandblasting to increase the surface roughness, heat treatment to correct the shape to ensure flatness, acid etching to remove the surface oxide scale, cleaning and drying for standby use;
[0009] Step 2), coating preparation: preparing a ruthenium titanium active solution, wherein the ruthenium titanium active solution contains a specified amount of ethyl cellulose;
[0010] Step 3), coating the ruthenium titanium active solution obtained in step 2) on the surface of the titanium substrate treated in step 1), drying after each coating, and then sintering at high temperature, repeating the coating, drying and sintering process multiple times until the solution is exhausted, thus obtaining a chlorine-evolving active anode.
[0011] Furthermore, in step 1), the sand mold for sandblasting is brown corundum or white corundum, the surface roughness Ra of the titanium substrate after sandblasting is between 15 and 25 μm, and the sandblasting coverage is ≥70%.
[0012] Furthermore, in step 1), after the titanium substrate is sandblasted, the temperature of the heat treatment shaping process is controlled at 500-530° C., the shaping time is controlled at 1-3 hours, and the unevenness of the titanium substrate after heat treatment shaping does not exceed 0.4 mm.
[0013] Furthermore, in step 1), after the titanium substrate is subjected to shape correction treatment, acid etching is continued to remove the surface oxide scale. During the acid etching process, the oxalic acid concentration is 5-15%, and the boiling etching time is 1-3 hours.
[0014] Furthermore, in step 2), the ruthenium titanium active solution is an organic solution containing butyl titanate, ruthenium trichloride and ethyl cellulose, the metal ion molar ratio is Ru:Ti=1~4:6~9, the amount of ethyl cellulose added is 0.1~10 times the mass of metal ion ruthenium, and the total metal ion concentration of the active solution is 0.1~0.3 mol / L.
[0015] Furthermore, the solvent in the organic solution is one or more of n-butanol, isopropanol or anhydrous ethanol.
[0016] Furthermore, in step 3), the sintering temperature is 400-480° C., each sintering time is 10-30 minutes, and the last sintering time is 1-2 hours.
[0017] The beneficial effects of the present invention are as follows: compared with the prior art, the high catalytic activity chlorine-evolving titanium anode provided by the present invention uses ethyl cellulose (EC) as a template for pore formation when preparing the ruthenium titanium catalytic active layer, which provides more nucleation sites for the ruthenium source, slows down the generation of wide cracks in the coating after sintering, increases the load per unit area, and increases the effective catalytic active area. At the same time, the pores generated by ethyl cellulose during the sintering process are conducive to the coating effectively promoting the transmission and release of sintering stress. The present invention uses ethyl cellulose as a template, which is a non-toxic and biodegradable polymer that has strong solubility in organic solvents and has a small mass after carbonization. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 This is a SEM image of the chlorine-evolving active anode prepared in Example 1 of the present invention;
[0019] Figure 2 This is a comparison diagram of the LSV curves of the chlorine evolution active anode prepared in Example 1 of the present invention and the conventional chlorine evolution anode;
[0020] Figure 3 This is a comparison chart of the effective chlorine content of the chlorine evolution active anode prepared in Example 1 of the present invention and the conventional chlorine evolution anode. DETAILED DESCRIPTION
[0021] The present invention is further described below by specific examples, but these examples are only used to illustrate the present invention and are not used to limit the scope of the present invention.
[0022] A method for preparing a chlorine-evolving titanium anode with high catalytic activity, the preparation method comprising the following steps:
[0023] Step 1), pre-treating the surface of the titanium substrate: sandblasting to increase the surface roughness, heat treatment to correct the shape to ensure flatness, acid etching to remove the surface oxide scale, cleaning and drying for standby use;
[0024] Step 2), coating preparation: preparing a ruthenium titanium active solution, wherein the ruthenium titanium active solution contains a specified amount of ethyl cellulose;
[0025] Step 3), coating the ruthenium titanium active solution obtained in step 2) on the surface of the titanium substrate treated in step 1), drying after each coating, and then sintering at high temperature, repeating the coating, drying and sintering process multiple times until the solution is exhausted, thus obtaining a chlorine-evolving active anode.
[0026] Furthermore, in step 1), the sand mold for sandblasting is brown corundum or white corundum, the surface roughness Ra of the titanium substrate after sandblasting is between 15 and 25 μm, and the sandblasting coverage is ≥70%.
[0027] Furthermore, in step 1), after the titanium substrate is sandblasted, the temperature of the heat treatment shaping process is controlled at 500-530° C., the shaping time is controlled at 1-3 hours, and the unevenness of the titanium substrate after heat treatment shaping does not exceed 0.4 mm.
[0028] Furthermore, in step 1), after the titanium substrate is subjected to shape correction treatment, acid etching is continued to remove the surface oxide scale. During the acid etching process, the oxalic acid concentration is 5-15%, and the boiling etching time is 1-3 hours.
[0029] Furthermore, in step 2), the ruthenium titanium active solution is an organic solution containing butyl titanate, ruthenium trichloride and ethyl cellulose, the metal ion molar ratio is Ru:Ti=1~4:6~9, the amount of ethyl cellulose added is 0.1~10 times the mass of metal ion ruthenium, and the total metal ion concentration of the active solution is 0.1~0.3 mol / L.
[0030] Furthermore, the solvent in the organic solution is one or more of n-butanol, isopropanol or anhydrous ethanol.
[0031] Furthermore, in step 3), the sintering temperature is 400-480° C., each sintering time is 10-30 minutes, and the last sintering time is 1-2 hours.
[0032] Comparative Example
[0033] 1. Titanium substrate pretreatment
[0034] Brown corundum was selected to sandblast the titanium substrate surface, with a sandblasting coverage of 80%, until the surface roughness Ra of the titanium substrate was between 15 and 18 μm. The sandblasted titanium substrate was placed in a 510℃ heat-shaped treatment for 1 hour, and the unevenness of the titanium substrate was 0.3 mm. The heat-shaped titanium substrate was placed in a 5% oxalic acid concentration and boiled for 1 hour to remove the surface oxide scale. After the end, it was rinsed with clean water and dried for use.
[0035] 2. Preparation of conventional chlorine evolution anode
[0036] A conventional ruthenium titanium solution was prepared, specifically, 1g of ruthenium trichloride and 2.5g of butyl titanate were dissolved in 30mL of n-butanol solution and stirred evenly. The conventional ruthenium titanium solution was coated on the surface of the pretreated titanium substrate, dried after each coating, and then placed in a 400°C sintering furnace for 10min high-temperature sintering, taken out and naturally cooled to room temperature, and the above coating and sintering steps were repeated. After the last coating, it was placed in a 400°C sintering furnace for high-temperature sintering for 1h to obtain a conventional chlorine evolution anode.
[0037] Example 1
[0038] A method for preparing a high catalytic activity chlorine-evolving titanium anode specifically comprises the following steps:
[0039] 1. Titanium substrate pretreatment
[0040] Brown corundum was selected to sandblast the titanium substrate surface, with a sandblasting coverage of 80%, until the surface roughness Ra of the titanium substrate was between 15 and 18 μm. The sandblasted titanium substrate was placed in a 510℃ heat-shaped treatment for 1 hour, and the unevenness of the titanium substrate was 0.3 mm. The heat-shaped titanium substrate was placed in a 5% oxalic acid concentration and boiled for 1 hour to remove the surface oxide scale. After the end, it was rinsed with clean water and dried for use.
[0041] 2. Preparation of chlorine-evolving active anode
[0042] The ruthenium titanium active solution was prepared, specifically, 1g of ruthenium trichloride, 2.5g of butyl titanate and 0.5g of ethyl cellulose (EC) were dissolved in 30mL of n-butanol solution and stirred evenly. The ruthenium titanium active solution was coated on the surface of the pretreated titanium substrate, dried after each coating, and then placed in a 400°C sintering furnace for 10min high-temperature sintering, taken out and naturally cooled to room temperature, and the above coating and sintering steps were repeated. After the last coating, it was placed in a 400°C sintering furnace for 1h of high-temperature sintering to obtain a chlorine-evolving active anode.
[0043] Figure 1 This is a SEM image of the chlorine evolution active anode successfully prepared in Example 1. It can be seen that the cracks on the surface of the anode are small, and the stable stacking morphology can increase the catalytic active sites, thereby improving its chlorine evolution catalytic performance.
[0044] Figure 2 Curve 1 and curve 2 are LSV curves of the chlorine evolution active anode and the conventional chlorine evolution anode prepared in Example 1. It can be clearly seen that the chlorine evolution potential of the chlorine evolution active anode is significantly lower than that of the conventional chlorine evolution anode, and the chlorine evolution active anode exhibits more excellent electrocatalytic performance.
[0045] Figure 3 This is a comparison chart of the effective chlorine content of the chlorine evolution active anode prepared in Example 1 and the conventional chlorine evolution anode. The chlorine evolution active anode prepared in Example 1 exhibits excellent chlorine evolution performance, which may be due to its larger chlorine evolution active area.
[0046] Example 2
[0047] A method for preparing a high catalytic activity chlorine-evolving titanium anode specifically comprises the following steps:
[0048] 1. Titanium substrate pretreatment
[0049] White corundum was selected to sandblast the titanium substrate surface, with a sandblasting coverage of 85%, until the surface roughness Ra of the titanium substrate was between 18 and 22 μm. The sandblasted titanium substrate was placed in a 520°C heat-shaped treatment for 2 hours, and the unevenness of the titanium substrate was 0.2 mm. The heat-shaped titanium substrate was placed in a 10% oxalic acid concentration and boiled for 2 hours to remove the surface oxide scale. After the end, it was rinsed with clean water and dried for use.
[0050] 2. Preparation of chlorine-evolving active anode
[0051] The ruthenium titanium active solution was prepared by dissolving 1.5g of ruthenium trichloride, 3g of butyl titanate and 1g of ethyl cellulose (EC) in 50mL of isopropanol solution and stirring evenly. The ruthenium titanium active solution was coated on the surface of the pretreated titanium substrate, dried after each coating, and then placed in a 450°C sintering furnace for 20min of high-temperature sintering, taken out and naturally cooled to room temperature, and the above coating and sintering steps were repeated. After the last coating, it was placed in a 450°C sintering furnace for high-temperature sintering for 1.5h to obtain a chlorine-evolving active anode.
[0052] Example 3
[0053] A method for preparing a high catalytic activity chlorine-evolving titanium anode specifically comprises the following steps:
[0054] 1. Titanium substrate pretreatment
[0055] White corundum was selected to sandblast the titanium substrate surface, with a sandblasting coverage of 90%, until the surface roughness Ra of the titanium substrate was between 20 and 25 μm. The sandblasted titanium substrate was placed in a 530°C heat correction treatment for 3 hours, and the unevenness of the titanium substrate was 0.1 mm. The heat-corrected titanium substrate was placed in a 15% oxalic acid concentration and boiled for acid etching for 3 hours to remove the surface oxide scale, and then rinsed with clean water and dried for use.
[0056] 2. Preparation of chlorine-evolving active anode
[0057] The ruthenium titanium active solution was prepared, specifically, 2g of ruthenium trichloride, 3.5g of butyl titanate and 2g of ethyl cellulose (EC) were dissolved in 80mL of anhydrous ethanol solution and stirred evenly. The ruthenium titanium active solution was coated on the surface of the pretreated titanium substrate, dried after each coating, and then placed in a 480°C sintering furnace for 25min high-temperature sintering, taken out and naturally cooled to room temperature, and the above coating and sintering steps were repeated. After the last coating, it was placed in a 480°C sintering furnace for high-temperature sintering for 2h to obtain a chlorine-evolving active anode.
[0058] The above implementation modes are only used to illustrate the present invention, but not to limit the present invention. Ordinary technicians in the relevant technical field can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, all equivalent technical solutions also belong to the scope of the present invention. The patent protection scope of the present invention should be defined by the claims.
Claims
1. A method for preparing a high catalytic activity chlorine-evolving titanium anode, characterized in that: The preparation method comprises the following steps: Step 1), pre-treating the surface of the titanium substrate: sandblasting to increase the surface roughness, heat treatment to correct the shape to ensure flatness, acid etching to remove the surface oxide scale, cleaning and drying for standby use; Step 2), coating preparation: preparing a ruthenium titanium active solution, wherein the ruthenium titanium active solution contains a specified amount of ethyl cellulose; Step 3), coating the ruthenium titanium active solution obtained in step 2) on the surface of the titanium substrate treated in step 1), drying after each coating, and then sintering at high temperature, repeating the coating, drying and sintering process multiple times until the solution is exhausted, thus obtaining a chlorine-evolving active anode.
2. The method for preparing a high catalytic activity chlorine-evolving titanium anode according to claim 1, characterized in that: In step 1), the sand mold for sandblasting is brown corundum or white corundum, the surface roughness Ra of the titanium substrate after sandblasting is between 15 and 25 μm, and the sandblasting coverage is ≥70%.
3. The method for preparing a high catalytic activity chlorine-evolving titanium anode according to claim 1, characterized in that: In step 1), after the titanium substrate is sandblasted, the temperature of the heat treatment shaping process is controlled at 500-530° C., the shaping time is controlled at 1-3 hours, and the unevenness of the titanium substrate after heat treatment shaping does not exceed 0.4 mm.
4. The method for preparing a high catalytic activity chlorine-evolving titanium anode according to claim 1, characterized in that: In step 1), after the titanium substrate is subjected to shape correction treatment, acid etching is continued to remove the surface oxide scale. During the acid etching process, the oxalic acid concentration is 5-15%, and the boiling etching time is 1-3 hours.
5. The method for preparing a high catalytic activity chlorine-evolving titanium anode according to claim 1, characterized in that: In step 2), the ruthenium titanium active solution is an organic solution containing butyl titanate, ruthenium trichloride and ethyl cellulose, the metal ion molar ratio is Ru:Ti=1~4:6~9, the amount of ethyl cellulose added is 0.1~10 times the mass of metal ion ruthenium, and the total metal ion concentration of the active solution is 0.1~0.3 mol / L.
6. The method for preparing a high catalytic activity chlorine-evolving titanium anode according to claim 5, characterized in that: The solvent in the organic solution is one or more of n-butanol, isopropanol or anhydrous ethanol.
7. The method for preparing a high catalytic activity chlorine-evolving titanium anode according to claim 1, characterized in that: In step 3), the sintering temperature is 400-480° C., each sintering time is 10-30 minutes, and the last sintering time is 1-2 hours.