Composition for spinning, intelligent temperature control fiber as well as preparation method and application of intelligent temperature control fiber
By uniformly dispersing the phase change capsules on the fiber wires, forming a spinning composition with a 'mutton skewer' structure, the problem of easy shedding of phase change fibers and complex preparation process is solved, the flexibility and breathability of the fibers are improved, and the wearability is enhanced Comfort, simplified process, and has great industrial application prospects.
Patent Information
- Application Number
- CN202310570823.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-19
- Publication Date
- 2024-11-22
AI Technical Summary
Existing phase-change fibers are prone to fall off during use and cleaning, resulting in poor breathability and moisture permeability of the fabric, and complex preparation process, high cost and low efficiency.
Using a spinning composition, including solvents, polymers and phase change capsules, the phase change capsules are uniformly dispersed on the fiber wires through centrifugal spinning technology to form a 'mutton skewers' structure to enhance the flexibility and breathability of the fibers.
It solves the problem that phase change materials are prone to fall off, improves the flexibility and breathability of the fiber membrane, enhances wearable comfort, simplifies the preparation process, reduces costs, and has a great prospect of industrial application.
Smart Images

Figure CN118996655A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of spinning, and in particular to a spinning composition and intelligent temperature-control fiber, and a preparation method and application thereof. Background Art
[0002] Fiber is an indispensable material in our daily life, especially in the field of wearable fabrics. Traditional textiles can only achieve temperature control effects by changing the thickness of the textiles and the quality of the still air in the textiles. However, its preparation technology has the defects of complex process and poor flexibility, especially the resulting textiles lack effective temperature control ability. With the improvement of people's living standards, developing high-performance functional fibers to solve the shortcomings of the above-mentioned traditional fibers is a feasible strategy. Among them, phase change materials are favored because they can release or store a large amount of energy during the phase change process and effectively control the temperature of the surrounding environment. Therefore, the phase change fibers obtained by combining phase change material technology and fiber textile technology have become a research hotspot.
[0003] At present, the preparation methods of phase change fibers mainly include direct filling method, direct coating method and spinning method. Among them, the simple direct filling method and direct coating method will lead to the intrinsic defects of poor air permeability and moisture permeability of the fabric. The phase change material is easily detached during the actual use and cleaning of the fabric, which will reduce the comfort and thermal insulation performance of the fabric. Compared with the above methods, the spinning method can integrate the phase change material into the fiber, which can greatly improve the morphological stability of PCMs in the fiber without affecting the air permeability and moisture permeability of the fiber membrane. At present, there are many kinds of spinning methods for preparing phase change fibers, but most methods have the characteristics of complex spinning equipment, high cost and low efficiency. Centrifugal spinning is a method for preparing fibers by spraying and stretching polymer solutions or melts under the action of supergravity fields and high-pressure cyclones. The diameter of the prepared fibers ranges from tens of nanometers to tens of microns, and has the characteristics of small diameter, light weight and large specific surface area. In the production of micro / nano fibers, compared with other spinning technologies, centrifugal spinning technology has advantages that cannot be ignored, such as high spinning efficiency and low cost. Summary of the invention
[0004] The purpose of the present invention is to overcome the above problems existing in the prior art and to provide a spinning composition and an intelligent temperature-control fiber and a preparation method and application thereof.
[0005] In order to achieve the above-mentioned object, the first aspect of the present invention provides a spinning composition, which comprises a solvent, a polymer and a phase change capsule;
[0006] Wherein, the phase change capsule comprises a packaging shell material and a phase change core material encapsulated in the packaging shell material;
[0007] Wherein, at the spinning temperature, the polymer is miscible with the solvent and the encapsulating shell material is immiscible with the solvent.
[0008] A second aspect of the present invention provides a method for preparing fibers, the method comprising: spinning the above composition.
[0009] The third aspect of the present invention provides a fiber prepared by the above method.
[0010] A fourth aspect of the present invention provides application of the above-mentioned fiber in flexible intelligent temperature regulation.
[0011] Through the above technical solution, the following beneficial effects can be achieved:
[0012] 1. The present invention adds phase change capsules to the spinning composition. The flexible intelligent temperature-control fiber obtained after spinning is further evenly dispersed on the fiber filaments through centrifugal spinning technology and firmly bonded to the fiber filaments, thereby solving the defect that the phase change material in the existing phase change fiber is easy to fall off.
[0013] 2. Compared with other phase change fibers, the fiber with the "mutton skewers" structure obtained by the preparation method of the present invention not only greatly increases the flexibility of the fiber membrane, but also increases the air permeability of the fiber membrane and the comfort of wearing the fiber membrane. The phase change fiber shows great application potential.
[0014] 3. The present invention adopts a centrifugal spinning process. Compared with other processes, the equipment is simple, no high-voltage electric field is required, the operation is simple, the efficiency is high, and it has great industrial application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 This is a scanning electron microscope image of the flexible intelligent temperature-control fiber with a "mutton skewer-like" structure obtained in Example 1;
[0016] Figure 2 This is a scanning electron microscope image of the flexible intelligent temperature-control fiber with a "mutton skewer-like" structure obtained in Example 2;
[0017] Figure 3 This is a scanning electron microscope image of the flexible intelligent temperature-control fiber with a "mutton skewer-like" structure obtained in Example 3;
[0018] Figure 4 The fiber membrane temperature of Example 5 changes with time;
[0019] Figure 5 The temperature below the fiber membrane of Example 1, Example 5 and Comparative Example 2 changes with the ambient temperature. DETAILED DESCRIPTION
[0020] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0021] A first aspect of the present invention provides a spinning composition, the composition comprising a solvent, a polymer and a phase change capsule;
[0022] Wherein, the phase change capsule comprises a packaging shell material and a phase change core material encapsulated in the packaging shell material;
[0023] Wherein, at the spinning temperature, the polymer is miscible with the solvent and the encapsulating shell material is immiscible with the solvent. The polymer is the same as or different from the encapsulating shell material, preferably different. Preferably, the polymer is miscible with the solvent means that the solubility of the polymer in the solvent at the spinning temperature is greater than or equal to 200 g / L. Preferably, the immiscible with the encapsulating shell material means that the solubility of the encapsulating shell material in the solvent at the spinning temperature is less than 10 g / L. The spinning temperature is generally 20-100°C, preferably 30-90°C.
[0024] In the present invention, in order to make the polymer easier to spin into silk, the degree of polymerization of the polymer is 1500-3000, which can be 1500, 1600, 1700, 1800, 1900, 2000, 2100, 2200, 2300, 2400, 2500, 2600, 2700, 2800, 2900, 3000 or a range formed by two of the above values and a value within the range.
[0025] In the present invention, in order to further make the phase change capsules evenly dispersed on the fiber filaments and firmly bonded to the fiber filaments, and increase the flexibility, air permeability and comfort of the obtained fiber membrane, the average cross-sectional diameter of the phase change capsules is 0.2-50 μm, which can be 0.2 μm, 0.4 μm, 0.6 μm, 0.8 μm, 1 μm, 3 μm, 5 μm, 7 μm, 9 μm, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, 150 μm, 160 μm, 170 μm, 180 μm, 190 μm, 210 μm, 220 μm, 230 μm, 240 μm, 250 μm, 260 μm, 270 μm, 280 μm, 290 μm, 300 μm, 350 μm, 30 ... 30μm, 35μm, 40μm, 45μm, 50μm or the range formed by two of the above values and the value within the range, the length is 0.2-50μm, and can be 0.2μm, 0.4μm, 0.6μm, 0.8μm, 1μm, 3μm, 5μm, 7μm, 9μm, 10μm, 15μm, 20μm, 25μm, 30μm, 35μm, 40μm, 45μm, 50μm or the range formed by two of the above values and the value within the range. Preferably, the phase change temperature of the phase change capsule is 0-100°C, which can be 0°C, 10°C, 20°C, 30°C, 40°C, 50°C, 60°C, 70°C, 80°C, 90°C, 100°C or any two of the above values in the range and the value within the range, and the phase change latent heat is 10-300J / g, which can be 10J / g, 30J / g, 50J / g, 70J / g, 90J / g, 110J / g, 130J / g, 150J / g, 170J / g, 190J / g, 220J / g, 240J / g, 260J / g, 280J / g, 300J / g or any two of the above values in the range and the value within the range. "Phase change temperature" refers to the critical temperature at which the phase change capsule changes from solid to liquid, and the test method is differential scanning calorimetry. "Latent heat of phase change" refers to the heat absorbed by a unit mass of phase change capsules when it changes from solid to liquid under isothermal and isobaric conditions. The test method is differential scanning calorimetry. The specific method of differential scanning calorimetry is: take 5-10 mg of sample and put it into a crucible, and then put the crucible and reference sample into the sample chamber of the DSC. Keep it at 100℃ for three minutes, and then cool it down to 0℃ at a cooling rate of 5℃ / min. After keeping it at 0℃ for 3 minutes, heat it up to 100℃ at a heating rate of 5℃ / min.
[0026] In the present invention, in order to further increase the flexibility, air permeability and comfort of the obtained fiber membrane, the weight ratio of the encapsulating shell material to the phase change core material is 1:1-5, and can be 1:1, 1:2, 1:3, 1:4, 1:5 or the range formed by any two of the above values and the value within the range. Preferably, the wall thickness of the encapsulating shell material is 0.05-10 μm.
[0027] In the present invention, in order to facilitate subsequent spinning, the weight ratio of the solvent to the polymer is 1:0.01-5, and can be 1:0.01, 1:0.05, 1:0.1, 1:0.15, 1:0.2, 1:0.25, 1:0.3, 1:0.4, 1:0.5, 1:0.6, 1:0.7, 1:0.8, 1:0.9, 1:1, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5, 1:4, 1:4.5, 1:5 or a range formed by any two of the above values and a value within the range. Preferably, the weight ratio of the solvent to the phase change capsule is 1:0.25-18, which can be 1:0.25, 1:0.3, 1:0.4, 1:0.5, 1:0.6, 1:0.7, 1:0.8, 1:0.9, 1:1, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5, 1:4, 1:4.5, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, 1:11, 1:12, 1:13, 1:14, 1:15, 1:16, 1:17, 1:18 or a range formed by any two of the above values and a value within the range, which can form a liquid environment and allow the solvent to evaporate in time during the subsequent spinning.
[0028] In the present invention, the solvent is a volatile reagent commonly used in the art, which is compatible with the polymer but incompatible with the encapsulating shell material at the spinning temperature, and is preferably at least one of dimethylformamide, dimethylacetamide, dimethyl sulfoxide, phenol, chloroform, acetone, methanol, toluene, water and carbon tetrachloride.
[0029] In the present invention, the polymer is a polymer commonly used in the art for preparing fibers, preferably at least one of polyvinyl alcohol, polyethylene, polypropylene, polylactic acid, cellulose acetate, polyvinyl chloride, polyvinyl acetal, polyester and polyurethane.
[0030] In the present invention, the encapsulation shell material is a material commonly used in the art that can encapsulate the phase change core material and is insoluble in solvents, preferably at least one of polyurea, polyacrylate, polyvinylidene fluoride, polyurethane, epoxy resin, urea-formaldehyde resin, polystyrene, gelatin, modified silica and titanium dioxide. The modified silica is formed by polymerization in the process of preparing the phase change capsule, and is a polymer polymerized into a long chain, not an inorganic silica.
[0031] In the present invention, the phase change core material is a common phase change material in the art, preferably at least one of saturated aliphatic hydrocarbons, fatty alcohols, fatty acids and hydrated inorganic salts. More preferably, the saturated aliphatic hydrocarbon is C 10 -C 40 At least one of the alkanes can also be a mixture, such as paraffin.
[0032] In the present invention, in order to further improve the bonding strength, flexibility and air permeability of the fiber, the composition may include polyvinyl alcohol, water and polyacrylate / saturated aliphatic hydrocarbon phase change capsules, or polyvinyl alcohol, water and polyacrylate / fatty alcohol phase change capsules, or polylactic acid, chloroform and modified silica / saturated aliphatic hydrocarbon phase change capsules, or polylactic acid, chloroform and modified silica / fatty alcohol phase change capsules, or polyvinyl chloride, tetrahydrofuran / cyclohexanone mixed solvent and urea-formaldehyde resin / hydrated inorganic salt phase change capsules, or polyethylene terephthalate, dimethylformamide and epoxy resin / (fatty alcohol+fatty acid) phase change capsules.
[0033] In the present invention, as described above, the phase change capsules can be at least one of polyacrylate / saturated aliphatic hydrocarbon phase change capsules, polyacrylate / fatty alcohol phase change capsules, modified silica / saturated aliphatic hydrocarbon phase change capsules, modified silica / fatty alcohol phase change capsules, urea-formaldehyde resin / hydrated inorganic salt phase change capsules, and epoxy resin / (fatty alcohol+fatty acid) phase change capsules, preferably polyacrylate / saturated aliphatic hydrocarbon phase change capsules or modified silica / saturated aliphatic hydrocarbon phase change capsules.
[0034] In the present invention, the preparation method of the phase change capsule is not limited, and the phase change core material can be encapsulated in the phase change shell material, preferably by spray drying, interfacial polymerization, emulsion polymerization or sol-gel method.
[0035] In a specific embodiment of the present invention, the modified silica / phase change paraffin phase change capsule is prepared by interfacial polymerization, and the specific preparation process may include: weighing a mixture of paraffin and ethyl orthosilicate in a weight ratio of 1:0.1-2, mixing and stirring at a stirring rate of 150-250rpm in a constant temperature water bath at 35-55°C for 25-35min to form a uniform mixed solution. The mixed solution is poured into a 150-250ml aqueous solution in which the weight ratio of water to octoxynol (emulsifier) is 1:0.001-0.1, and emulsified at 800-1200rpm in a constant temperature water bath at 25-45°C for 1-3h. After emulsification is completed, the speed is reduced to 200-400rpm, and a few drops of 0.8-1.2mol / L dilute hydrochloric acid are added to the emulsion to adjust the pH to 8-9. Subsequently, the reaction was continued for 45-52 h in a constant temperature water bath at 35-55° C. and a stirring rate of 150-250 rpm to obtain phase change capsules.
[0036] In the present invention, the polyacrylate / eicosane phase change capsule is prepared by interfacial polymerization, and the specific preparation process may include: weighing 150-250 ml of water and octoxynol (emulsifier) (the weight ratio of water to emulsifier is 1: 0.001-0.1), and mixing them thoroughly to obtain a uniform aqueous solution. Then weigh a mixture of acrylic acid monomer, eicosane solution and an optional initiator (such as azobisisobutyronitrile), the weight ratio of which is 1: 0.1-10. Pour the mixture into a clean and dry four-necked flask. If an initiator is added, stir rapidly at 30-50° C. so that the initiator can be dissolved. The weight ratio of the initiator to the acrylic acid monomer is less than or equal to 0.1, preferably 0.005-0.1. Then slowly add the aqueous solution to the four-necked flask and stir at high speed for 20-40 minutes to make the solution a stable emulsion. The emulsion system is heated to 60-80°C at a heating rate of 0.8-1.2°C / min, kept warm for reaction for 2-6 hours, and then the temperature is raised to 75-95°C and kept warm for reaction for 1-3 hours, thereby obtaining phase change capsules.
[0037] In the present invention, in order to enhance the interaction between the polymer and the phase change capsule, the composition further includes a surfactant.
[0038] In the present invention, in order to further increase the interaction between the polymer and the phase change capsules, the weight ratio of the solvent to the surfactant is 1:0.001-0.5, and can be 1:0.001, 1:0.002, 1:0.003, 1:0.004, 1:0.005, 1:0.006, 1:0.007, 1:0.008, 1:0.009, 1:0.01, 1:0.02, 1:0.03, 1:0.04, 1:0.05, 1:0.06, 1:0.07, 1:0.08, 1:0.09, 1:0.1, 1:0.2, 1:0.3, 1:0.4, 1:0.5 or the range formed by any two of the above values and the value within the range.
[0039] In the present invention, the surfactant is a common agent in the art that can increase the interaction between the polymer and the phase change capsule, preferably at least one of stearic acid, sodium alkylbenzene sulfonate, fatty acid glyceride, isomeric alcohol polyoxyethylene ether, alkylphenol polyoxyethylene ether, fatty alcohol ether sulfate, alkyl alcohol amide, amino acid-based surfactant, quaternary ammonium salt surfactant and sulfated castor oil.
[0040] In the present invention, in order to improve the anti-oxidation, antibacterial, flame retardant, strength and thermal stability of the fiber, the composition further includes an auxiliary agent, and the weight ratio of the auxiliary agent to the solvent is less than or equal to 1, preferably less than or equal to 0.05, and more preferably 0.01-0.05. Preferably, the auxiliary agent is at least one of an antioxidant, an antibacterial agent, a cross-linking agent, a flame retardant and a thermal stabilizer.
[0041] For example, antioxidants, antibacterial agents, crosslinking agents, flame retardants and heat stabilizers can all be common choices in the art. The antioxidant can be antioxidant 1010, and the antibacterial agent can be trichlorocarbamide.
[0042] According to a preferred embodiment of the present invention, the composition is only composed of the above ingredients. The fiber with a "mutton skewers" structure can be prepared by the above composition.
[0043] A second aspect of the present invention provides a method for preparing fibers, the method comprising: spinning using the above composition.
[0044] In the present invention, in order to increase the flexibility, air permeability and comfort of the obtained fiber membrane, the spinning method is centrifugal spinning.
[0045] In the present invention, in order to further increase the flexibility, air permeability and comfort of the obtained fiber membrane, the aperture of the spinneret in the centrifugal spinning is 0.06-4 mm; more preferably, the rotation speed of the spinning head in the centrifugal spinning is 1000-20000 rpm.
[0046] The third aspect of the present invention provides a fiber prepared by the above method.
[0047] The fourth aspect of the present invention provides the application of the above-mentioned fiber in flexible intelligent temperature regulation. The fiber can be prepared into at least one of clothing, medical dressings, external protection materials for electronic devices and energy storage materials, and used for functional fabrics, thermal management and energy storage.
[0048] The present invention will be described in detail below through examples. In the following examples, the size of the obtained fiber membrane is 5×5 cm and the thickness is 2 mm.
[0049] The preparation process of modified silica / phase-change paraffin phase-change capsules includes: weighing a mixture of paraffin and ethyl orthosilicate with a weight ratio of 1:1 and mixing and stirring at a stirring rate of 200 rpm in a constant temperature water bath at 45°C for 30 minutes to form a uniform mixed solution. The mixed solution is poured into a 200 ml aqueous solution with a weight ratio of water to octoxynol (emulsifier) of 1:0.01, and emulsified at 1000 rpm in a constant temperature water bath at 35°C for 2 hours. After the emulsification is completed, the speed is reduced to 300 rpm, and a few drops of 1 mol / L dilute hydrochloric acid are added to the emulsion to adjust the pH to 8.5. Subsequently, the constant temperature water bath at 45°C and the stirring rate of 200 rpm are maintained for 48 hours to obtain phase-change capsules. The shell material is modified silica and the core material is paraffin as measured by infrared spectroscopy. The diameter and length of the phase change capsule measured by electron microscopy are 1 μm and 1 μm respectively, and the wall thickness measured by transmission electron microscopy is 0.2 μm. The phase change temperature is 44.4℃ and the latent heat of phase change is 210 J / g. The latent heat of phase change of paraffin is 260 J / g. The weight ratio of the encapsulating shell material to the phase change core material in the phase change capsule is 1:4.2, and the formula is the latent heat of phase change capsule / latent heat of paraffin.
[0050] The preparation process of polyacrylate / eicosane phase change capsules includes: weighing 200 ml of water and octoxynol (emulsifier) (the weight ratio of water to emulsifier is 1:0.01), and mixing them thoroughly to obtain a uniform aqueous solution. Then weigh a mixture of acrylic acid monomer, eicosane solution and initiator (azobisisobutyronitrile) in a weight ratio of 1:5:0.01. Pour the mixture into a clean and dry four-necked flask and stir rapidly at 40°C to dissolve the initiator. Then slowly add the aqueous solution to the four-necked flask and stir at high speed for half an hour to make the solution a stable emulsion. Raise the temperature of the emulsion system to 75°C at a heating rate of 1°C / min, keep warm for 4 hours, and then raise the temperature to 85°C for 2 hours to obtain a phase change capsule. The shell material is polyacrylate and the core material is eicosane as measured by infrared spectroscopy. The average diameter and length of the phase change capsules measured by electron microscopy are 1 μm and 1 μm, respectively. The wall thickness is 0.2 μm, the phase change temperature is 36.4°C, and the latent heat of phase change is 150.8 J / g as measured by transmission electron microscopy. The latent heat of phase change of eicosane is 230 J / g. The weight ratio of the encapsulated shell material to the phase change core material in the phase change capsule is 1:1.85, and the formula is the latent heat of phase change capsule / latest heat of eicosane.
[0051] The test method for fiber antibacterial properties is: GB / T 20944.3-2008 "Evaluation of antibacterial properties of textiles Part 3: Oscillation method".
[0052] The test method for the antioxidant capacity of fibers is: T / CCTA 20102-2023 "Determination and evaluation of antioxidant capacity of textiles-DHHP and ABTS methods".
[0053] Polyvinyl alcohol (degree of polymerization 2500) Source: Kuraray International Trading (Shanghai) Co., Ltd.;
[0054] Polyacrylate (DP 1500-2500) Source: Wacker Chemie AG;
[0055] Eicosane source: Aladdin Chemical Reagent Co., Ltd.;
[0056] Alkyl alcohol amide Source: Jinan Beiyate Chemical Technology Co., Ltd.;
[0057] Source of trichlorocarbamide: Shandong Aoyou Biotechnology Co., Ltd.
[0058] Paraffin source: Shanghai Myril Biochemical Technology Co., Ltd.;
[0059] Isotriol polyoxyethylene ether 1309 Source: Zhengzhou Yihe Fine Chemicals Co., Ltd., brand: RO21190S;
[0060] Polylactic acid (DP 2500) Source: COFCO Group;
[0061] Antioxidant 1010 Source: Shuangtai New Materials Co., Ltd.
[0062] Source of tridecylphenol polyoxyethylene 18 ether: Hai'an Petrochemical Plant, Jiangsu Province, brand number: 466875.
[0063] Example 1
[0064] (1) Polyvinyl alcohol, polyacrylate / eicosane phase change capsules, water, alkyl alcohol amide and antimicrobial agent in a mass ratio of 15:35:48:1:1 are weighed to prepare a uniform centrifugal spinning solution, wherein the antimicrobial agent is trichlorocarbamide.
[0065] (2) The speed of the centrifugal spinning machine was set to 3000 rpm, and the spinneret diameter was set to 0.5 mm. The spinning solution was placed in the cavity of the spinning head, and the cavity temperature was maintained at 90°C. After the motor was turned on, a flexible intelligent temperature-controlled fiber membrane with a "lamb skewer" structure was obtained on the collector. The test results of the obtained fiber properties are shown in Table 1.
[0066] Example 2
[0067] (1) Weigh polyvinyl alcohol, polyacrylate / eicosane phase change capsules, water, alkyl alcohol amide and antibacterial agent in a mass ratio of 10:40:48:1:1 to prepare a uniform centrifugal spinning solution, wherein the antibacterial agent is trichlorocarbamide.
[0068] (2) The speed of the centrifugal spinning machine was set to 3000 rpm, and the spinneret diameter was set to 0.5 mm. The spinning solution was placed in the cavity of the spinning head, and the cavity temperature was maintained at 90°C. After the motor was turned on, a flexible intelligent temperature-controlled fiber membrane with a "lamb skewer" structure was obtained on the collector. The test results of the obtained fiber properties are shown in Table 1.
[0069] Example 3
[0070] (1) Polyvinyl alcohol, polyacrylate / eicosane phase change capsules, water, alkyl alcohol amide and antimicrobial agent in a mass ratio of 5:45:48:1:1 are weighed to prepare a uniform centrifugal spinning solution, wherein the antimicrobial agent is trichlorocarbamide.
[0071] (2) The speed of the centrifugal spinning machine was set to 3000 rpm, and the spinneret diameter was set to 0.5 mm. The spinning solution was placed in the cavity of the spinning head, and the cavity temperature was maintained at 90°C. After the motor was turned on, a flexible intelligent temperature-controlled fiber membrane with a "lamb skewer" structure was obtained on the collector. The test results of the obtained fiber properties are shown in Table 1.
[0072] Example 4
[0073] The method of Example 1 was followed, except that the diameter of the phase change capsule was changed to 3 μm (the emulsification speed of 1000 rpm was changed to 800 rpm when preparing the phase change capsule). The test results of the obtained fiber properties are shown in Table 1.
[0074] Example 5
[0075] (1) Weigh polyvinyl alcohol, modified silica / phase change paraffin wax phase change capsules, deionized water, isomeric tridecanol polyoxyethylene ether and antibacterial agent in a mass ratio of 15:35:48:1:1 to prepare a uniform centrifugal spinning solution. The antibacterial agent is trichlorocarbamide.
[0076] (2) The speed of the centrifugal spinning machine was set to 3000 rpm, and the spinneret diameter was set to 0.5 mm. The spinning solution was placed in the cavity of the spinning head, and the cavity temperature was maintained at 90°C. After the motor was turned on, a flexible intelligent temperature-controlled fiber membrane with a "lamb skewer" structure was obtained on the collector. The test results of the obtained fiber properties are shown in Table 1.
[0077] Example 6
[0078] The method of Example 5 was followed, except that the rotation speed of the centrifugal spinning machine was changed to 6000 rpm. The test results of the obtained fiber properties are shown in Table 1.
[0079] Example 7
[0080] (1) Weigh polylactic acid, modified silica / phase change paraffin wax phase change capsules, dichloromethane, alkylphenol polyoxyethylene ether and antibacterial agent in a mass ratio of 15:35:48:1:1 to prepare a uniform centrifugal spinning solution, wherein the antibacterial agent is trichlorocarbamide.
[0081] (2) The speed of the centrifugal spinning machine was set to 3000 rpm, and the spinneret diameter was set to 0.5 mm. The spinning solution was placed in the cavity of the spinning head, and the cavity temperature was maintained at 30°C. After the motor was turned on, a flexible intelligent temperature-controlled fiber membrane with a "mutton skewer" structure was obtained on the collector. The test results of the obtained fiber properties are shown in Table 1.
[0082] Example 8
[0083] The method of Example 7 was followed, except that the antibacterial agent was replaced with antioxidant 1010. The test results of the obtained fiber properties are shown in Table 1.
[0084] Example 9
[0085] The method of Example 8 was followed, except that the diameter of the spinneret hole was changed to 0.7 mm. The test results of the obtained fiber properties are shown in Table 1.
[0086] Example 10
[0087] (1) Weigh polylactic acid, modified silica / phase change paraffin phase change capsules, dichloromethane, alkylphenol polyoxyethylene ether and antioxidant in a mass ratio of 12:28:56:2:2 to prepare a uniform centrifugal spinning solution. The antioxidant is antioxidant 1010.
[0088] (2) The speed of the centrifugal spinning machine is set to 3000 rpm, and the diameter of the spinneret hole is set to 0.5 mm. The spinning solution is placed in the cavity of the spinning head, and the cavity temperature is maintained at 30°C. After the motor is turned on, a flexible intelligent temperature-controlled fiber membrane with a "mutton skewer" structure is obtained on the collector.
[0089] Embodiment 11
[0090] The method of Example 1 was followed, except that when preparing the polyacrylate / eicosane phase change capsules, the weight ratio of polyacrylate to eicosane was 1:6. The test results of the obtained fiber properties are shown in Table 1.
[0091] Comparative Example 1
[0092] According to the method of Example 1, the difference is that no polyacrylate / eicosane phase change capsule is added, and polyvinyl alcohol, water, alkyl alcohol amide and antibacterial agent are directly prepared into a centrifugal spinning solution for centrifugal spinning. The obtained fiber membrane is immersed in molten eicosane, and a phase change fiber membrane is prepared by a conventional coating method. The test results of the obtained fiber membrane performance are shown in Table 1.
[0093] Comparative Example 2
[0094] The method of Example 1 is followed, except that no polyacrylate is added, and the centrifugal spinning solution prepared with polyvinyl alcohol, eicosane, water, alkyl alcohol amide and antibacterial agent is directly spun. The test results of the obtained fiber properties are shown in Table 1.
[0095] Comparative Example 3
[0096] The method of Comparative Example 1 was followed, except that the obtained fiber membrane was not immersed in molten eicosane. The test results of the obtained fiber properties are shown in Table 1.
[0097] Comparative Example 4
[0098] The method of Example 1 is different from that of preparing polyacrylate / eicosane phase change capsules first, and polyvinyl alcohol, polyacrylate, eicosane, water, alkyl alcohol amide and antibacterial agent are directly mixed to prepare a spinning solution for spinning. The test results of the obtained fiber properties are shown in Table 1.
[0099] Test Case
[0100] (1) Testing of fiber properties
[0101] Test method for latent heat of phase change: Differential scanning calorimetry. Take 8 mg of sample and put it into a crucible, then put the crucible and reference sample into the sample chamber of DSC. Keep it at 100℃ for three minutes, then cool it down to 0℃ at a cooling rate of 5℃ / min. After keeping it at 0℃ for 3 minutes, heat it up to 100℃ at a heating rate of 5℃ / min.
[0102] Phase transition temperature test method: Differential scanning calorimetry. The steps are the same as above.
[0103] The bonding strength between the fiber and the phase change capsule is determined by rubbing, twisting and bending the fiber membrane by hand.
[0104] Fiber membrane flexibility: judge by squeezing, stretching, twisting and bending the fiber membrane by hand.
[0105] Fiber membrane air permeability: GB / T 5453-1997 “Determination of air permeability of textile fabrics”. The test results are shown in Table 1.
[0106] Table 1
[0107]
[0108]
[0109] Note: Strong: +++++, Stronger: ++++, Medium: +++, Weaker: ++, Weak: +, - means non-existent.
[0110] (2) Temperature control capability test
[0111] A thermocouple was placed on a foam board, and the thermocouple was covered with the fiber membrane obtained in the above examples and comparative examples and placed under sunlight. The ambient temperature and the temperature of the film below the fiber membrane were recorded by a collector within 400 seconds (the temperature was automatically recorded every 1 second), and the maximum temperature, minimum temperature and average temperature within the 400 seconds were obtained, as shown in Table 2. Among them, the temperature of the fiber membrane of Example 5 changes with time as shown in Table 2. Figure 4 The temperature below the fiber membrane of Example 1, Example 5 and Comparative Example 2 changes with the ambient temperature as shown in Figure 5 The results show that the temperature difference below the fiber membrane obtained in the embodiment of the present invention is small, and the difference with the ambient temperature is large, showing a relatively good temperature control ability.
[0112] Table 2
[0113]
[0114]
[0115] It can be seen from the results in Table 1 that the "kebab" structure constructed by the embodiment of the present invention not only greatly increases the flexibility of the fiber membrane, but also increases the air permeability of the fiber membrane, and increases the wearing comfort and temperature control ability of the fiber membrane.
[0116] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A spinning composition, characterized in that The composition includes a solvent, a polymer and phase change capsules; Wherein, the phase change capsule comprises a packaging shell material and a phase change core material encapsulated in the packaging shell material; Wherein, at the spinning temperature, the polymer is miscible with the solvent and the encapsulating shell material is immiscible with the solvent.
2. The composition according to claim 1, wherein The degree of polymerization of the polymer is 1500-3000; And / or, the phase change capsules have an average cross-sectional diameter of 0.2-50 μm and a length of 0.2-50 μm; And / or, the phase change temperature of the phase change capsule is 0-100°C, and the phase change latent heat is 10-300 J / g; And / or, the weight ratio of the packaging shell material to the phase change core material is 1:1-5; And / or, the wall thickness of the packaging shell material is 0.05-10 μm; And / or, the weight ratio of the solvent, the polymer and the phase change capsule is 1:0.2-5:0.25-18.
3. The composition according to claim 1 or 2, wherein The solvent is at least one of dimethylformamide, dimethylacetamide, dimethyl sulfoxide, phenol, chloroform, acetone, methanol, toluene, water and carbon tetrachloride; and / or, the polymer is at least one of polyvinyl alcohol, polyethylene, polypropylene, polylactic acid, cellulose acetate, polyvinyl chloride, polyvinyl acetal, polyester and polyurethane; and / or, the packaging shell material is at least one of polyurea, polyacrylate, polyvinylidene fluoride, polyurethane, epoxy resin, urea-formaldehyde resin, polystyrene, gelatin, modified silicon dioxide and titanium dioxide; And / or, the phase change core material is at least one of saturated aliphatic hydrocarbons, fatty alcohols, fatty acids and hydrated inorganic salts.
4. The composition according to claim 1 or 2, wherein The composition also includes a surfactant; Preferably, the weight ratio of the solvent to the surfactant is 1:0.001-0.
5.
5. The composition according to claim 4, wherein The surfactant is at least one of stearic acid, sodium alkylbenzene sulfonate, fatty acid glyceride, isomeric alcohol polyoxyethylene ether, alkylphenol polyoxyethylene ether, fatty alcohol ether sulfate, alkylolamide, amino acid-based surfactant, quaternary ammonium salt surfactant and sulfated castor oil.
6. The composition according to claim 1 or 2, wherein The composition also includes an auxiliary agent; Preferably, the weight ratio of the auxiliary agent to the solvent is less than or equal to 1; Preferably, the auxiliary agent is at least one of an antioxidant, an antibacterial agent, a cross-linking agent, a flame retardant and a heat stabilizer.
7. A method for preparing fiber, characterized in that: The method comprises: spinning using the composition described in any one of claims 1 to 6.
8. The method according to claim 7, wherein: The spinning method is centrifugal spinning; Preferably, the aperture of the spinneret in the centrifugal spinning is 0.06-4 mm; Preferably, the rotation speed of the spinning head in the centrifugal spinning is 1000-20000 rpm.
9. Fibers prepared by the method of claim 7 or 8.
10. Application of the fiber according to claim 9 in flexible intelligent temperature control.