Self-suspending film-coated proppant and preparation method thereof
By forming a resin coating layer and a hydrophobic layer on the surface of the aggregate, and using the cross-linking reaction of sodium alginate and chitosan to form a micro-nano structure, the failure problem of traditional proppants under high temperature and high pressure conditions is solved, and the self-improvement is achieved Suspension and efficient flow diversion improve the mining efficiency of oil and gas wells.
Patent Information
- Application Number
- CN202411335847.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-24
- Publication Date
- 2024-11-22
AI Technical Summary
Traditional coated proppants are prone to fall off or fail under high temperature, high pressure and high mineralization formation conditions, resulting in a reduced support effect and may adhere in oil and gas wells with high closing pressure, seriously affecting the flow diversion ability of the cracks.
Using a self-suspended coating proppant, a resin coating layer and a hydrophobic layer are formed on the surface of the aggregate and bubbles are embedded in the resin coating layer, and a micro-nano structure is formed by cross-linking reaction between sodium alginate and chitosan. Improve the durability and flow diversion capability of proppants.
Self-suspended under the condition of no thickener is achieved, the durability and mining efficiency of the proppant are improved, and the resistance to closed pressure and the flow-driving performance are enhanced, so that the flow-driving ability of the proppant remains stable for a long time.
Smart Images

Figure CN118997718A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of fluid mining, and in particular to a self-suspended film-coated proppant and a preparation method thereof. Background Art
[0002] In the process of exploitation of fluid minerals (gas, oil, hot water, etc.), it is often necessary to stimulate the flow of hydrocarbons via hydraulic fracturing. The term "fracturing" refers to a method of pumping fluid into a well until the pressure is increased to a level sufficient to break up the underground geological formations containing trapped materials. This process results in cracks and fractures that destroy the underlying layers to allow hydrocarbon products to be carried to the well bore at a significantly higher rate. However, unless the pressure is maintained, the newly formed orifice closes. In order to open the path and maintain the path, a supporting agent or "proppant" is injected with the hydraulic fluid to produce the support required to maintain the orifice. When the fracture is formed, the proppant is transferred in the slurry by releasing the hydraulic pressure, and the proppant forms a fill or support for keeping the open fracture.
[0003] The fracturing process uses a high-pressure, large-displacement pump on the ground. Utilizing the principle of liquid pressure transmission, a liquid with a certain viscosity (usually referred to as fracturing fluid) is injected into the reservoir at a pressure greater than the absorptive capacity of the reservoir, and the pressure in the wellbore is gradually increased, thereby creating high pressure at the bottom of the well. When this pressure is greater than the ground stress near the well wall and the tensile strength of the formation rock, cracks are generated in the formation near the bottom of the well. Fracturing fluid with proppants (also known as sand-carrying fluid) is continuously injected, and the cracks extend forward and are filled with proppants. After the well is shut down, the cracks are closed on the proppants, thereby forming cracks filled with proppants with certain geometric dimensions and high conductivity in the formation near the bottom of the well (fluids such as oil can be diverted out from the gaps in the proppants), so that the well can achieve the purpose of increasing production and injection.
[0004] Although traditional coated proppants have the advantages of improving the anti-crushing ability of proppants and improving the conductivity of fractures in hydraulic fracturing construction, under certain extreme formation conditions, such as high temperature, high pressure, high mineralization, etc., the chemical stability of the coating layer may be affected, causing the coating layer to fall off or fail, thereby affecting the support effect. In addition, in oil and gas wells with high closure pressure, traditional coated proppants may adhere, resulting in a serious decrease in the conductivity of the fracture. Summary of the invention
[0005] The purpose of the present invention is to overcome the deficiencies in the prior art and provide a self-suspending coated proppant and a preparation method thereof, which realizes self-suspension without a thickener and improves the durability and mining efficiency of the proppant.
[0006] The present invention is achieved through the following technical solutions: on the one hand, a self-suspending coated proppant is provided, which is composed of aggregate, a resin coating layer coated on the outer surface of the aggregate, and a hydrophobic layer; the aggregate and the resin coating layer are combined through a micro-nano layer, and bubbles are embedded in the interior of the resin coating layer.
[0007] Furthermore, the added amount of the resin coating layer accounts for 5-15wt% of the aggregate; and the added amount of the hydrophobic layer accounts for 1.5-3wt% of the resin coating layer.
[0008] Furthermore, the resin coating layer is made by mixing fluorosilicone copolymer resin, aliphatic isocyanate curing agent, terminal hydroxyl silicone oil, foaming agent and catalyst in a mass ratio of 1:5-15:1-5:0.5-5:0.1-1.
[0009] Furthermore, the fluorosilicone copolymer resin is a synthetic resin mixed with a fluororesin and an organic silicone resin, and has a temperature resistance of >220 degrees and a hardness of >3H.
[0010] Furthermore, the aliphatic isocyanate curing agent is any one of hexamethylene diisocyanate biuret, hexamethylene diisocyanate trimer and isophorone diisocyanate trimer.
[0011] Furthermore, the terminal hydroxyl silicone oil is a low molecular weight terminal hydroxyl polydimethylsiloxane with a viscosity between 25 and 30 CP.
[0012] Furthermore, the foaming agent is a physical foaming agent or a chemical foaming agent; the physical foaming agent is CO2 or N2; the chemical foaming agent is azodicarbonamide (ADC) or N,N-dimethyl-N,N-dinitrosopentamethylenetetramine (DPT).
[0013] A method for preparing the self-suspending coated proppant is also provided, comprising the following steps:
[0014] Step S1: prepare materials according to the above formula;
[0015] Step S2: formation of Wiener layer;
[0016] Adding sodium alginate powder into a deionized water solution, stirring the mixture at 30-35°C at a speed of 550-650 r / min, and forming a sodium alginate solution through swelling and dissolution;
[0017] Dissolving chitosan powder in acetic acid solution and stirring until completely dissolved to form a chitosan solution;
[0018] The chitosan solution is then added to the sodium alginate solution, and the mixture is concentrated by vigorous stirring. The aggregate is then evenly dispersed in the mixed solution, and the carboxyl groups in the sodium alginate molecules interact with the amino groups in the chitosan molecules to form a Wiener layer with a Wiener structure on the surface of the aggregate.
[0019] Step S3: preparing a resin coating layer;
[0020] The fluorosilicone copolymer resin, the fatty isocyanate curing agent, the terminal hydroxyl silicone oil, the foaming agent and the catalyst are mixed evenly according to the prescribed amount to form a resin coating solution; the resin coating solution is evenly sprayed on the surface of the wiener layer obtained in step S2 by a coating machine to form a uniform wet film layer; and then the wiener layer is placed in an oven for curing at a heating rate of 5-10°C / min, the curing time is 8-12h, and the curing temperature is 60°C to 120°C, until the resin coating layer is completely cross-linked and cured;
[0021] Step S4: preparation of a hydrophobic layer;
[0022] The surface of the resin coating layer obtained in step S3 is coated with a fluorosilane coupling agent solution, and then cured, washed, and dried to obtain the obtained product.
[0023] Furthermore, in step S2, the mass ratio of chitosan to sodium alginate is 1-5:5-1.
[0024] Furthermore, in step S4, the fluorosilane coupling agent solution is prepared by dissolving 1-5% of the fluorosilane coupling agent in anhydrous ethanol and stirring the mixture thoroughly.
[0025] Beneficial Effects
[0026] The present invention uses resin to encapsulate aggregates, and a hydrophobic layer is coated on the surface of the resin coating layer, thereby increasing the contact area between sand particles, thereby improving the ability of the proppant to resist closure pressure; in addition, the resin coating layer can wrap up crushed small pieces and silt, etc., reducing the migration between particles and the chance of clogging the pores, thereby improving the fracture conductivity.
[0027] The self-suspended coated proppant prepared by the present invention adopts sodium alginate and chitosan to undergo cross-linking reaction to form a micro-nano structure. The existence of the micro-nano structure gives the coated proppant a deformable function, increases its contact area, and can effectively prevent the proppant from being embedded in soft formations.
[0028] The self-suspending coated proppant prepared by the present invention can generate a certain number of bubbles inside the resin coating layer by adding a foaming agent in the coating layer. The bubbles embedded in the resin coating layer can reduce the specific gravity of the proppant to a certain extent. In addition, thanks to the micro-nano structure formed by the reaction of sodium alginate and chitosan, the density of the proppant is further reduced, and the self-suspending performance of the coated proppant is improved, so that the proppant has high conductivity, no fracturing fluid residue, the proppant is not easy to break, the conductivity can be kept stable for a long time, and the effective period is long. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is the SEM spectrum of the micro-nano structure prepared by the present invention; DETAILED DESCRIPTION
[0030] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0031] Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. The experimental methods without specific conditions in the following examples are usually carried out under conventional conditions or according to the conditions recommended by the manufacturer. Unless otherwise specified, all percentages, ratios, proportions or parts are by weight.
[0032] Unless otherwise specified, the reagents and raw materials used in the examples and comparative examples of the present invention can be obtained through commercial channels.
[0033] Example 1
[0034] A method for preparing a self-suspending coated proppant comprises the following steps:
[0035] Step S1: preparing materials;
[0036] High-purity, high-hardness alumina ceramic particles are used as proppant aggregates, with a particle size range of 0.5-1.0mm;
[0037] Sodium alginate powder: Use sodium alginate powder with a purity of 99%;
[0038] Chitosan powder: choose chitosan powder with a deacetylation degree greater than 90%;
[0039] Fluorosilicone copolymer resin, temperature resistance reaches 250℃, hardness is 4H;
[0040] The hydroxy-terminated silicone oil is a low molecular weight hydroxy-terminated polydimethylsiloxane with a viscosity of 28CP;
[0041] Catalyst: organic tin catalyst is selected;
[0042] Fluorosilane coupling agent: select perfluoropolyether fluorosilane coupling agent;
[0043] Solvent, DPG solvent;
[0044] The mass ratio of fluorosilicone copolymer resin: aliphatic isocyanate curing agent: terminal hydroxyl silicone oil: blowing agent: catalyst is 1:10:3:2:0.5;
[0045] Step S2: formation of Wiener layer;
[0046] Slowly add 5 grams of sodium alginate powder to 100 milliliters of deionized water, stirring while adding; stir at 600r / min for 2 hours in a constant temperature water bath at 30°C until the sodium alginate is completely swollen and dissolved to form a uniform and transparent sodium alginate solution. Add 3 grams of chitosan powder to 50mL of 1% acetic acid solution; stir at 550r / min for 3 hours at room temperature of 25°C until the chitosan is completely dissolved to form a light yellow chitosan solution. Slowly add the prepared chitosan solution to the sodium alginate solution, stirring at 800r / min with a powerful mixer, and continue stirring for 1 hour to fully mix and concentrate the two solutions to form a mixed solution. Disperse 20g of alumina ceramic particles evenly in the mixed solution and keep stirring vigorously to allow the aggregate to be fully immersed in the mixed solution. During the stirring process, the carboxyl groups in the sodium alginate molecules interact with the amino groups in the chitosan molecules to gradually form a dense Wiener layer on the surface of the aggregate. Continue stirring for 30 minutes to ensure that the Wiener layer is evenly and firmly attached to the surface of the aggregate.
[0047] Step S3: preparing a resin coating layer;
[0048] Weigh 0.13 g of fluorosilicone copolymer resin, 1.30 g of fatty isocyanate curing agent, 0.39 g of terminal hydroxyl silicone oil, 0.26 g of azodicarbonamide (ADC) and 0.06 g of catalyst and mix them evenly to form a resin coating solution; use a coating machine to evenly spray the resin coating solution on the surface of the Wiener layer obtained in step S2 to form a uniform wet film layer; then place it in an oven for curing at a heating rate of 8°C / min, the curing time is 10 hours, and the curing temperature is 90°C, until the resin coating layer is completely cross-linked and cured;
[0049] Step S4: preparation of a hydrophobic layer;
[0050] Dissolve 0.04 g of fluorosilane coupling agent in an appropriate amount of DPG solvent to form a fluorosilane coupling agent solution; use a coating machine or a dip coating method to evenly coat the fluorosilane coupling agent solution on the surface of the resin coating layer, place it in an oven for curing treatment at a curing temperature of 98° C. and a curing time of 18 hours, then wash and dry to obtain the product.
[0051] Example 2
[0052] A method for preparing a self-suspending coated proppant comprises the following steps:
[0053] Step S1: preparing materials;
[0054] High-purity, high-hardness alumina ceramic particles are used as proppant aggregates, with a particle size range of 0.5-1.0mm;
[0055] Sodium alginate powder: Use sodium alginate powder with a purity of 99%;
[0056] Chitosan powder: choose chitosan powder with a deacetylation degree greater than 90%;
[0057] Fluorosilicone copolymer resin, temperature resistance reaches 250℃, hardness is 4H;
[0058] The hydroxy-terminated silicone oil is a low molecular weight hydroxy-terminated polydimethylsiloxane with a viscosity of 28CP;
[0059] Catalyst: organic tin catalyst is selected;
[0060] Fluorosilane coupling agent: select perfluoropolyether fluorosilane coupling agent;
[0061] Solvent, DPG solvent;
[0062] The mass ratio of fluorosilicone copolymer resin: aliphatic isocyanate curing agent: terminal hydroxyl silicone oil: blowing agent: catalyst is 1:15:5:4:1;
[0063] Step S2: formation of Wiener layer;
[0064] Slowly add 5 grams of sodium alginate powder to 100 milliliters of deionized water while stirring; stir at 600 r / min for 2 hours in a constant temperature water bath at 30°C until the sodium alginate is completely swollen and dissolved to form a uniform and transparent sodium alginate solution. Add 12.5 grams of chitosan powder to 50 mL of 1% acetic acid solution; stir at 550 r / min for 3 hours at room temperature until the chitosan is completely dissolved to form a light yellow chitosan solution. Slowly add the prepared chitosan solution to the sodium alginate solution while stirring with a powerful mixer at 800 r / min, and continue stirring for 1 hour to fully mix and concentrate the two solutions to form a mixed solution. Disperse 20g of alumina ceramic particles evenly in the mixed solution and keep stirring vigorously to allow the aggregate to be fully immersed in the mixed solution. During the stirring process, the carboxyl groups in the sodium alginate molecules interact with the amino groups in the chitosan molecules to gradually form a dense Wiener layer on the surface of the aggregate. Continue stirring for 30 minutes to ensure that the Wiener layer is evenly and firmly attached to the surface of the aggregate.
[0065] Step S3: preparing a resin coating layer;
[0066] Weigh 0.13 g of fluorosilicone copolymer resin, 1.95 g of aliphatic isocyanate curing agent, 0.65 g of terminal hydroxyl silicone oil, 0.52 g of N,N-dimethyl-N,N-dinitrosopentamethylenetetramine (DPT) and 0.13 g of catalyst and mix them evenly to form a resin coating solution; use a coating machine to evenly spray the resin coating solution on the surface of the Wiener layer obtained in step S2 to form a uniform wet film layer; then place it in an oven for curing at a heating rate of 8°C / min, the curing time is 8 hours, and the curing temperature is 95°C, until the resin coating layer is completely cross-linked and cured;
[0067] Step S4: preparation of a hydrophobic layer;
[0068] Dissolve 0.06g of fluorosilane coupling agent in an appropriate amount of DPG solvent to form a fluorosilane coupling agent solution; use a coating machine or a dip coating method to evenly coat the fluorosilane coupling agent solution on the surface of the resin coating layer, place it in an oven, and perform a curing treatment at a curing temperature of 100°C for 12 hours, then wash and dry to obtain the product.
[0069] Example 3
[0070] A method for preparing a self-suspending coated proppant comprises the following steps:
[0071] Step S1: preparing materials;
[0072] High-purity, high-hardness alumina ceramic particles are used as proppant aggregates, with a particle size range of 0.5-1.0mm;
[0073] Sodium alginate powder: Use sodium alginate powder with a purity of 99%;
[0074] Chitosan powder: choose chitosan powder with a deacetylation degree greater than 90%;
[0075] Fluorosilicone copolymer resin, temperature resistance reaches 250℃, hardness is 4H;
[0076] The hydroxy-terminated silicone oil is a low molecular weight hydroxy-terminated polydimethylsiloxane with a viscosity of 28CP;
[0077] Catalyst: organic tin catalyst is selected;
[0078] Fluorosilane coupling agent: select perfluoropolyether fluorosilane coupling agent;
[0079] Solvent, DPG solvent;
[0080] The mass ratio of fluorosilicone copolymer resin: aliphatic isocyanate curing agent: terminal hydroxyl silicone oil: blowing agent: catalyst is 1:8:2:1.5:0.3;
[0081] Step S2: formation of Wiener layer;
[0082] Slowly add 5 grams of sodium alginate powder to 100 milliliters of deionized water while stirring; stir at 600r / min for 2 hours in a constant temperature water bath at 30°C until the sodium alginate is completely swollen and dissolved to form a uniform and transparent sodium alginate solution. Add 3 grams of chitosan powder to 50mL of 1% acetic acid solution; stir at 550r / min for 3 hours at room temperature until the chitosan is completely dissolved to form a light yellow chitosan solution. Slowly add the prepared chitosan solution to the sodium alginate solution while stirring with a powerful mixer at 800r / min, and continue stirring for 1 hour to fully mix and concentrate the two solutions to form a mixed solution. Disperse 20g of alumina ceramic particles evenly in the mixed solution and keep stirring vigorously to allow the aggregate to be fully immersed in the mixed solution. During the stirring process, the carboxyl groups in the sodium alginate molecules interact with the amino groups in the chitosan molecules to gradually form a dense Wiener layer on the surface of the aggregate. Continue stirring for 30 minutes to ensure that the Wiener layer is evenly and firmly attached to the surface of the aggregate.
[0083] Step S3: preparing a resin coating layer;
[0084] Weigh 0.14 g of fluorosilicone copolymer resin, 1.05 g of fatty isocyanate curing agent, 0.28 g of terminal hydroxyl silicone oil, 0.23 g of azodicarbonamide (ADC) and 0.042 g of catalyst and mix them evenly to form a resin coating solution; use a coating machine to evenly spray the resin coating solution on the surface of the Wiener layer obtained in step S2 to form a uniform wet film layer; then place it in an oven and cure it at a heating rate of 8°C / min. The curing time is 8 hours and the curing temperature is 95°C until the resin coating layer is completely cross-linked and cured. The mass of the obtained resin coating layer is 2 g.
[0085] Step S4: preparation of a hydrophobic layer;
[0086] Dissolve 0.05g of fluorosilane coupling agent in an appropriate amount of DPG solvent to form a fluorosilane coupling agent solution; use a coating machine or a dip coating method to evenly coat the fluorosilane coupling agent solution on the surface of the resin coating layer, place it in an oven for curing treatment at a curing temperature of 95°C and a curing time of 10 hours, then wash and dry to obtain the product.
[0087] On the basis of the above technical solution, the foaming agent can also be replaced by a physical foaming agent, such as filling CO2 or N2.
[0088] Example 4
[0089] A method for preparing a self-suspending coated proppant comprises the following steps:
[0090] Step S1: preparing materials;
[0091] High-purity, high-hardness alumina ceramic particles are used as proppant aggregates, with a particle size range of 0.5-1.0mm;
[0092] Sodium alginate powder: Use sodium alginate powder with a purity of 99%;
[0093] Chitosan powder: choose chitosan powder with a deacetylation degree greater than 90%;
[0094] Fluorosilicone copolymer resin, temperature resistance reaches 250℃, hardness is 4H;
[0095] The hydroxy-terminated silicone oil is a low molecular weight hydroxy-terminated polydimethylsiloxane with a viscosity of 28CP;
[0096] Catalyst: organic tin catalyst is selected;
[0097] Fluorosilane coupling agent: select perfluoropolyether fluorosilane coupling agent;
[0098] Solvent, DPG solvent;
[0099] The mass ratio of fluorosilicone copolymer resin: aliphatic isocyanate curing agent: terminal hydroxyl silicone oil: foaming agent: catalyst is 1:12:4:3:0.8;
[0100] Step S2: formation of Wiener layer;
[0101] Slowly add 5 grams of sodium alginate powder to 100 milliliters of deionized water while stirring; stir at 600 r / min for 2 hours in a constant temperature water bath at 30°C until the sodium alginate is completely swollen and dissolved to form a uniform and transparent sodium alginate solution. Add 12.5 grams of chitosan powder to 50 mL of 1% acetic acid solution; stir at 550 r / min for 3 hours at room temperature until the chitosan is completely dissolved to form a light yellow chitosan solution. Slowly add the prepared chitosan solution to the sodium alginate solution while stirring with a powerful mixer at 800 r / min, and continue stirring for 1 hour to fully mix and concentrate the two solutions to form a mixed solution. Disperse 20g of alumina ceramic particles evenly in the mixed solution and keep stirring vigorously to allow the aggregate to be fully immersed in the mixed solution. During the stirring process, the carboxyl groups in the sodium alginate molecules interact with the amino groups in the chitosan molecules to gradually form a dense Wiener layer on the surface of the aggregate. Continue stirring for 30 minutes to ensure that the Wiener layer is evenly and firmly attached to the surface of the aggregate.
[0102] Step S3: preparing a resin coating layer;
[0103] Weigh 0.13 g of fluorosilicone copolymer resin, 1.58 g of hexamethylene diisocyanate biuret, 0.53 g of terminal hydroxyl silicone oil, 0.41 g of azodicarbonamide (ADC) and 0.11 g of a catalyst and mix them evenly to form a resin coating solution; use a coating machine to evenly spray the resin coating solution on the surface of the Wiener layer obtained in step S2 to form a uniform wet film layer; then place it in an oven for curing at a heating rate of 8°C / min, the curing time is 8 hours, and the curing temperature is 95°C, until the resin coating layer is completely cross-linked and cured;
[0104] Step S4: preparation of a hydrophobic layer;
[0105] Dissolve 0.08g of fluorosilane coupling agent in an appropriate amount of DPG solvent to form a fluorosilane coupling agent solution; use a coating machine or a dip coating method to evenly coat the fluorosilane coupling agent solution on the surface of the resin coating layer, place it in an oven, and perform a curing treatment at a curing temperature of 100°C for 12 hours, then wash and dry to obtain the product.
[0106] Comparative Example 1
[0107] A method for preparing a self-suspended coated proppant comprises the following steps: firstly, high-purity and high-hardness alumina ceramic particles are selected as proppant aggregates, and the particle size range is 0.5-1.0 mm; after coal gangue, clay, magnesium oxide powder and manganese dioxide powder are mixed in a certain proportion, they are lightly calcined at 800°C for 2 hours, and then ground to an average particle size of less than 50 μm; wherein the mass ratio of coal gangue to clay is 1:1, and the mass ratio of magnesium oxide powder to manganese dioxide powder is 1:2. The proppant aggregate is mixed with a small amount of adhesive in an appropriate amount of water, and a primary blank ball with a diameter of about 1.2-1.5 mm is formed by a rotary granulator; the coated powder is evenly sprayed on the surface of the primary blank ball, and the powder is tightly attached to the blank ball by rotary coating to form an intermediate blank ball. Silica sol is evenly sprayed on the surface of the intermediate blank ball, with a solid content of 30% to form a dense silica sol film layer with a thickness of about 10-20μm; the sprayed spherical proppant particles are dried at 100°C for 2 hours to remove moisture; and then sintered at 1200°C for 2 hours to make the silica sol film layer tightly combined with the coating layer and aggregate to form a solid coating structure, thereby obtaining a self-suspending coated proppant.
[0108] Effect Example
[0109] The following testing process was performed on Examples 1 to 4 and Comparative Example 1:
[0110] Take a 100ml test tube, add 80ml of clean water, then add 32g of the self-suspending film-coated proppant prepared in specific examples 1-4 and comparative example 1 (sand-liquid ratio 0.4), mix evenly, wait for the self-suspending film-coated proppant to be completely dispersed, shake well, make the self-suspending film-coated proppant completely suspended, put the test tube on the test tube rack, and record the time for its complete sedimentation. The results are shown in Table 1 below:
[0111] Table 1:
[0112]
[0113]
[0114] By comparing the experimental data of Examples 1-4 and the comparative example, it can be seen that the self-suspending coated proppant prepared by the present invention can generate a certain number of bubbles inside the resin coating layer by adding a foaming agent in the coating layer. The bubbles embedded in the resin coating layer can reduce the specific gravity of the proppant to a certain extent. In addition, thanks to the micro-nano structure formed by the reaction of sodium alginate and chitosan, the density of the proppant is further reduced, and the self-suspending performance of the coated proppant is improved, so that the proppant has high conductivity, no fracturing fluid residue, the proppant is not easy to break, the conductivity can remain stable for a long time, and the effective period is long.
[0115] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A self-suspending coated proppant, characterized in that: The self-suspended coated proppant is composed of aggregate, a resin coating layer coated on the outer surface of the aggregate, and a hydrophobic layer; the aggregate and the resin coating layer are combined through a micro-nano layer, and bubbles are embedded in the resin coating layer.
2. The self-suspending coated proppant according to claim 1, characterized in that: The added amount of the resin coating layer accounts for 5 to 15 wt % of the aggregate; the added amount of the hydrophobic layer accounts for 1.5 to 3 wt % of the resin coating layer.
3. The self-suspending coated proppant according to claim 1, characterized in that: The resin coating layer is prepared by mixing fluorine-silicon copolymer resin, aliphatic isocyanate curing agent, terminal hydroxyl silicone oil, foaming agent and catalyst in a mass ratio of 1:5-15:1-5:0.5-5:0.1-1.
4. The self-suspending coated proppant according to claim 3, characterized in that: The fluorosilicone copolymer resin is a synthetic resin mixed with fluororesin and silicone resin, and has a temperature resistance of more than 220° C. and a hardness of more than 3H.
5. The self-suspended coated proppant according to claim 3, characterized in that: The aliphatic isocyanate curing agent is any one of hexamethylene diisocyanate biuret, hexamethylene diisocyanate trimer and isophorone diisocyanate trimer.
6. The self-suspending coated proppant according to claim 3, characterized in that: The terminal hydroxyl silicone oil is a low molecular weight terminal hydroxyl polydimethylsiloxane with a viscosity between 25 and 30 CP.
7. The self-suspended coated proppant according to claim 3, characterized in that: The foaming agent is a physical foaming agent or a chemical foaming agent; the physical foaming agent is CO2 or N2; the chemical foaming agent is azodicarbonamide (ADC) or N,N-dimethyl-N,N-dinitrosopentamethylenetetramine (DPT).
8. A method for preparing the self-suspending coated proppant according to any one of claims 1 to 7, characterized in that: The following steps are involved: Step S1: prepare materials according to the above formula; Step S2: formation of Wiener layer; Adding sodium alginate powder into a deionized water solution, stirring the mixture at 30-35°C at a speed of 550-650 r / min, and forming a sodium alginate solution through swelling and dissolution; Dissolving chitosan powder in acetic acid solution and stirring until completely dissolved to form a chitosan solution; The chitosan solution is then added to the sodium alginate solution, and the mixture is concentrated by vigorous stirring. The aggregate is then evenly dispersed in the mixed solution, and the carboxyl groups in the sodium alginate molecules interact with the amino groups in the chitosan molecules to form a Wiener layer with a Wiener structure on the surface of the aggregate. Step S3: preparing a resin coating layer; The fluorosilicone copolymer resin, the fatty isocyanate curing agent, the terminal hydroxyl silicone oil, the foaming agent and the catalyst are mixed evenly according to the prescribed amount to form a resin coating solution; the resin coating solution is evenly sprayed on the surface of the wiener layer obtained in step S2 by a coating machine to form a uniform wet film layer; and then the wiener layer is placed in an oven for curing at a heating rate of 5-10°C / min, the curing time is 8-12h, and the curing temperature is 60°C to 120°C, until the resin coating layer is completely cross-linked and cured; Step S4: preparation of a hydrophobic layer; The surface of the resin coating layer obtained in step S3 is coated with a fluorosilane coupling agent solution, and then cured, washed, and dried to obtain the obtained product.
9. The method for preparing the self-suspending coated proppant according to claim 8, characterized in that: In step S2, the mass ratio of chitosan to sodium alginate is 1-5:5-1.
10. The method for preparing the self-suspending coated proppant according to claim 8, characterized in that: In step S4, the fluorosilane coupling agent solution is prepared by dissolving 1-5% of the fluorosilane coupling agent in anhydrous ethanol and stirring the mixture thoroughly.