Freezing sleep equipment with high heat preservation performance
By adopting a double-layer insulation structure and a modified foam insulation layer in the sleeping equipment, and using the combination of vacuum interlayer and foam insulation layer, the problem of insufficient insulation effect of the sleeping equipment under low temperature conditions is solved, and efficient energy is achieved Improved thermal insulation and safety.
Patent Information
- Application Number
- CN202411081964.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-22
AI Technical Summary
The existing sleeping equipment has poor insulation effect under low temperature conditions, resulting in high refrigeration energy consumption and a risk of frostbite. A sleeping equipment with high insulation performance is needed to reduce energy consumption and prevent frostbite.
A double-layer thermal insulation structure is adopted, wherein the first structural layer is a vacuum interlayer, and the second structural layer is filled with a modified foam insulation layer. The foam insulation layer is composed of polyether polyol, 2-fluorophenyl isocyanate, and aerogel microspheres. , barium sulfate, fluorinated graphite and water magnesite are composed of materials, and are foamed by modified composite fillers to form an efficient insulation layer.
It achieves higher insulation effect, wear resistance and tensile strength, effectively blocking environmental heat conduction, reducing refrigeration energy consumption, prevent frostbite and achieve energy conservation and emission reduction.
Smart Images

Figure CN118999072A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of cryosleep equipment, and in particular to cryosleep equipment with high heat preservation performance. Background Art
[0002] Cryosleep equipment, such as the Chinese patent announcement number CN213687436U, CN215724583U, etc., uses ultra-low temperature technology to directly contact the frozen objects through cryosleep liquid as a refrigerant. The frozen objects, such as aquatic products, meat, fruits and vegetables, are directly frozen and preserved in the cryosleep liquid within 6 to 30 minutes. The freezing temperature can be as low as -30°C. The cell membrane of the frozen object is not frozen and is in a slightly frozen state of the organism. The frozen and preserved aquatic products, meat, fruits and vegetables are then refrigerated to keep them fresh and fresh. Cryosleep equipment requires cryosleep liquid as a refrigerant, and the frozen objects are immersed in the cryosleep liquid to freeze them quickly. A large amount of cryosurgery liquid needs to be contained in the cryosurgery equipment, and the temperature of the cryosurgery liquid is usually below -30°C. Therefore, the cryosurgery equipment needs to be strictly insulated to block the heat conduction between the low-temperature cryosurgery liquid and the external working environment, to avoid low temperatures outside the cryosurgery equipment and frostbite the operators, and at the same time avoid increasing the refrigeration load and energy consumption of the cryosurgery equipment, so as to keep the cryosurgery liquid within the required temperature range in real time.
[0003] Current cryosleep equipment reduces heat conduction between cryosleep fluid and the external working environment as much as possible by adding an insulation layer in the interlayer between the double-layer insulation structure and the cryosleep fluid container. However, the insulation layer is generally made of polyurethane plastic for insulation. However, the current polyurethane plastic has a poor insulation effect on cryosleep fluid below -30°C.
[0004] Therefore, in view of the shortcomings of the prior art, it is necessary to provide a cryosleep device with high thermal insulation performance to solve the shortcomings of the prior art. Summary of the invention
[0005] The purpose of the present invention is to avoid the shortcomings of the prior art and provide a cryo-hibernation device with high thermal insulation performance. The cryo-hibernation device with high thermal insulation performance has good thermal insulation performance, thereby reducing refrigeration energy consumption and achieving energy saving and emission reduction.
[0006] The above-mentioned purpose of the present invention is achieved by the following technical measures:
[0007] A cryosleep device with high thermal insulation performance is provided, which comprises a main body and a accommodating liner for accommodating cryosleep liquid, wherein the accommodating liner is assembled inside the main body, and a double-layer insulation structure is arranged outside the accommodating liner, wherein the double-layer insulation structure comprises a first structure layer and a second structure layer, wherein the first structure layer is close to the accommodating liner, and the second structure layer is located outside the first structure layer, wherein the first structure layer is a vacuum interlayer, and a foam insulation layer is filled in the second structure layer.
[0008] The raw materials of the foamed thermal insulation layer contain polyether polyol, 2-fluorophenyl isocyanate, polyethylene glycol, aerogel microspheres, barium sulfate, fluorinated graphite, hydromagnesite, dimethyl silicone oil, N-bromosuccinimide, isopentane, water and tris[2.4-di-tert-butylphenyl]phosphite.
[0009] Preferably, the thermal conductivity of the foamed insulation layer is 0.0171 W / m·K to 0.0192 W / m·K.
[0010] Preferably, the closed cell ratio of the foamed thermal insulation layer is 96.15% to 96.99%.
[0011] Preferably, the average diameter of the pores of the foamed thermal insulation layer is 0.182 mm to 0.186 mm.
[0012] Preferably, the foam core density of the foam insulation layer is 0.226 g / cm 3 ~0.243g / cm 3 .
[0013] Preferably, the minimum thickness of the foam insulation layer is 10 mm to 30 mm.
[0014] In the foamed thermal insulation layer, by weight,
[0015] Polyether polyol: 40 parts;
[0016] 2-Fluorophenyl isocyanate: 18 to 28 parts;
[0017] Polyethylene glycol: 3 to 8 parts;
[0018] Aerogel microspheres: 8 to 12 parts;
[0019] Graphite fluoride: 1 to 2 parts;
[0020] Barium sulfate: 0.4 to 0.8 parts;
[0021] Hydromagnesite: 0.5 to 1 part;
[0022] Dimethyl silicone oil: 8 to 15 parts;
[0023] N-bromosuccinimide: 1 to 3 parts;
[0024] Isopentane: 8 to 10 parts;
[0025] Water: 1 to 3 parts;
[0026] Tris[2,4-di-tert-butylphenyl]phosphite: 0.2 to 0.4 parts.
[0027] In the foamed thermal insulation layer, by weight,
[0028] In the foamed thermal insulation layer, by weight,
[0029] Polyether polyol: 40 parts;
[0030] 2-Fluorophenyl isocyanate: 23 parts;
[0031] Polyethylene glycol: 7 parts;
[0032] Aerogel microspheres: 10.5 parts;
[0033] Graphite fluoride: 1.5 parts;
[0034] Barium sulfate: 0.6 parts;
[0035] Hydromagnesite: 0.7 parts;
[0036] Dimethyl silicone oil: 12 parts;
[0037] N-bromosuccinimide: 2.3 parts;
[0038] Isopentane: 9 parts;
[0039] Water: 2.5 parts;
[0040] Tris[2,4-di-tert-butylphenyl]phosphite: 0.3 parts.
[0041] Preferably, the method for preparing the foamed thermal insulation layer comprises the following steps:
[0042] S1, mixing polyether polyol, polyethylene glycol, dimethyl silicone oil, aerogel microspheres, graphite fluoride, barium sulfate, hydromagnesite, N-bromosuccinimide, water and tris[2,4-di-tert-butylphenyl]phosphite, and entering S2;
[0043] S2, add 2-fluorophenyl isocyanate, stir and mix to obtain an intermediate, and proceed to S3;
[0044] S3, adding isopentane to the intermediate to foam it to obtain a polyurethane foam semi-finished product, and then injecting the polyurethane foam semi-finished product into the second structural layer;
[0045] S4, ripening the accommodating liner, the double-layer insulation structure and the polyurethane foam semi-finished product as a whole to obtain the foam insulation layer.
[0046] Preferably, the method for preparing the foamed thermal insulation layer comprises the following steps:
[0047] S1, polyether polyol, polyethylene glycol, dimethyl silicone oil, aerogel microspheres, graphite fluoride, barium sulfate, hydromagnesite, N-bromosuccinimide, water and tris[2,4-di-tert-butylphenyl]phosphite, stirring at a stirring speed of 100 r / min to 120 r / min for 15 min to 30 min, and then entering S2;
[0048] S2, add 2-fluorophenyl isocyanate, stir at a stirring speed of 1000 r / min to 1200 r / min, stir for 15 min to 30 min to obtain an intermediate, and enter S3;
[0049] S3, adding isopentane to the intermediate, stirring for 7s to 10s and then foaming to obtain a polyurethane foam semi-finished product, and then adding the polyurethane foam semi-finished product into the second structural layer, and the volume ratio of the intermediate to the second structural layer is 1:25 to 28;
[0050] S4. Curing the accommodating liner, the double-layer insulation structure and the polyurethane foam semi-finished product as a whole at a curing temperature of 105° C. to 115° C. for a curing time of 18 h to 36 h to obtain the foam insulation layer.
[0051] The present invention provides a cryosleep device with high heat preservation performance, which is provided with a main body and a container for containing cryosleep liquid, the container is assembled inside the main body, and a double-layer insulation structure is provided outside the container, the double-layer insulation structure is provided with a first structure layer and a second structure layer, the first structure layer is close to the container, the second structure layer is located outside the first structure layer, the first structure layer is a vacuum interlayer, and a foam insulation layer is filled in the second structure layer; the raw materials of the foam insulation layer contain polyether polyol, 2-fluorophenyl isocyanate, polyethylene glycol, aerogel microspheres, barium sulfate, fluorinated graphite and hydromagnesite, dimethyl silicone oil, N-bromosuccinimide, isopentane, water and tris[2.4-di-tert-butylphenyl]phosphite. The cryosleep device of the present invention is heat-insulated by providing a double-layer insulation structure, wherein the first structure layer is a vacuum interlayer, and the second structure layer is filled with a foam insulation layer. The foamed insulation layer is modified by using a modified composite filler, and aerogel microspheres, barium sulfate, fluorinated graphite and hydromagnesite are introduced into the 2-fluorophenyl polyurethane system of the present invention, so that the foamed insulation layer has a higher level in terms of thermal insulation effect, wear resistance and tensile strength. The present invention effectively blocks the conduction of ambient heat to the cryosleep liquid through double insulation of the vacuum interlayer and the foamed insulation layer, prevents the outer wall of the cryosleep equipment from freezing the operator, and can also reduce refrigeration energy consumption, thereby achieving energy conservation and emission reduction. DETAILED DESCRIPTION
[0052] The technical solution of the present invention is further described in conjunction with the following examples. Unless otherwise specified, the raw materials used in the following examples are all commercially available products. BRIEF DESCRIPTION OF THE DRAWINGS
[0053] The present invention is further described with reference to the accompanying drawings, but the contents in the accompanying drawings do not constitute any limitation to the present invention.
[0054] Figure 1 A perspective view of a cryosleep device.
[0055] exist Figure 1 Including:
[0056] The main body 100 , the first structure layer 200 , the second structure layer 300 , and the accommodating liner 400 .
[0057] Example 1
[0058] A cryosleep device with high thermal insulation performance, such as Figure 1 As shown, a main body 100 and a containing liner 400 for containing cryosleep liquid are provided, the containing liner 400 is assembled inside the main body 100, and a double-layer insulation structure is provided outside the containing liner 400, and the double-layer insulation structure is provided with a first structure layer 200 and a second structure layer 300, the first structure layer 200 is close to the containing liner 400, and the second structure layer 300 is located outside the first structure layer 200, the first structure layer 200 is a vacuum interlayer, and a foam insulation layer is filled in the second structure layer 300.
[0059] The thermal conductivity of the foam insulation layer is 0.0171W / m·K to 0.0192W / m·K. The closed porosity of the foam insulation layer is 96.15% to 96.99%. The average diameter of the pores of the foam insulation layer is 0.182mm to 0.186mm. The foam core density of the foam insulation layer is 0.226g / cm 3 ~0.243g / cm 3 The minimum thickness of the foam insulation layer is 10 mm to 30 mm, and the thickness of the vacuum interlayer is 20 mm.
[0060] It should be noted that the foam insulation layer of the present invention has a small thermal conductivity and a small density, and the thickness of the foam insulation layer can be reduced while ensuring the insulation effect, thereby reducing the overall volume and weight of the cryosleep device.
[0061] The raw materials of the foaming insulation layer contain polyether polyol, 2-fluorophenyl isocyanate, polyethylene glycol, aerogel microspheres, barium sulfate, fluorinated graphite and hydromagnesite, dimethyl silicone oil, N-bromosuccinimide, isopentane, water and tris[2.4-di-tert-butylphenyl]phosphite.
[0062] In the foamed thermal insulation layer, by weight,
[0063] Polyether polyol: 40 parts;
[0064] 2-Fluorophenyl isocyanate: 18 to 28 parts;
[0065] Polyethylene glycol: 3 to 8 parts;
[0066] Aerogel microspheres: 8 to 12 parts;
[0067] Graphite fluoride: 1 to 2 parts;
[0068] Barium sulfate: 0.4 to 0.8 parts;
[0069] Hydromagnesite: 0.5 to 1 part;
[0070] Dimethyl silicone oil: 8 to 15 parts;
[0071] N-bromosuccinimide: 1 to 3 parts;
[0072] Isopentane: 8 to 10 parts;
[0073] Water: 1 to 3 parts;
[0074] Tris[2,4-di-tert-butylphenyl]phosphite: 0.2 to 0.4 parts.
[0075] The method for preparing the foamed thermal insulation layer comprises the following steps:
[0076] S1, polyether polyol, polyethylene glycol, dimethyl silicone oil, aerogel microspheres, graphite fluoride, barium sulfate, hydromagnesite, N-bromosuccinimide, water and tris[2,4-di-tert-butylphenyl]phosphite, stirring at a stirring speed of 100 r / min to 120 r / min for 15 min to 30 min, and then entering S2;
[0077] S2, add 2-fluorophenyl isocyanate, stir at a stirring speed of 1000 r / min to 1200 r / min, stir for 15 min to 30 min to obtain an intermediate, and enter S3;
[0078] S3, adding isopentane to the intermediate, stirring for 7s to 10s and then foaming to obtain a polyurethane foam semi-finished product, and then adding the polyurethane foam semi-finished product into the second structural layer, and the volume ratio of the intermediate to the second structural layer is 1:25 to 28;
[0079] S4. Curing the accommodating liner, the double-layer insulation structure and the polyurethane foam semi-finished product as a whole at a curing temperature of 105° C. to 115° C. for a curing time of 18 h to 36 h to obtain the foam insulation layer.
[0080] The cryosleep device is insulated by setting up a double-layer insulation structure, wherein the first structural layer is a vacuum interlayer, and the second structural layer is filled with a foam insulation layer. The foam insulation layer is modified by using a modified composite filler, and aerogel microspheres, barium sulfate, graphite fluoride and hydromagnesite are introduced into the 2-fluorophenyl polyurethane system of the present invention. The foam insulation layer has a higher level in terms of thermal insulation effect, wear resistance and tensile strength. The present invention effectively blocks the conduction of environmental heat to the cryosleep liquid through double insulation of the vacuum interlayer and the foam insulation layer, preventing the outer wall of the cryosleep device from freezing the operator, while also reducing refrigeration energy consumption and achieving energy conservation and emission reduction.
[0081] Example 2
[0082] A cryosleep device with high thermal insulation performance, other features are the same as those of Example 1, except that: the minimum thickness of the foam insulation layer is 20 mm.
[0083] In the foamed thermal insulation layer, by weight,
[0084] Polyether polyol: 40 parts;
[0085] 2-Fluorophenyl isocyanate: 18 parts;
[0086] Polyethylene glycol: 8 parts;
[0087] Aerogel microspheres: 8 parts;
[0088] Graphite fluoride: 1 part;
[0089] Barium sulfate: 0.4 parts;
[0090] Hydromagnesite: 0.5 parts;
[0091] Dimethyl silicone oil: 15 parts;
[0092] N-bromosuccinimide: 3 parts;
[0093] Isopentane: 10 parts;
[0094] Water: 1 part;
[0095] Tris[2,4-di-tert-butylphenyl]phosphite: 0.2 parts.
[0096] The method for preparing the foamed thermal insulation layer comprises the following steps:
[0097] The preparation method of the cryosleep device with high heat preservation performance is characterized by comprising the following steps:
[0098] S1, polyether polyol, polyethylene glycol, dimethyl silicone oil, aerogel microspheres, graphite fluoride, barium sulfate, hydromagnesite, N-bromosuccinimide, water and tris[2,4-di-tert-butylphenyl]phosphite, stirring at a stirring speed of 100 r / min for 15 min, and then entering S2;
[0099] S2, add 2-fluorophenyl isocyanate, stir at a stirring speed of 1000 r / min, stir for 15 min, obtain an intermediate, and enter S3;
[0100] S3, adding isopentane to the intermediate, stirring for 10 seconds and then foaming to obtain a polyurethane foam semi-finished product, and then putting the polyurethane foam semi-finished product into the second structural layer 300, and the volume ratio of the intermediate to the second structural layer 300 is 1:25;
[0101] S4. The lining 400, the double-layer insulation structure and the polyurethane foam semi-finished product are subjected to a curing temperature of 105° C. for 18 hours to obtain a foam insulation layer.
[0102] Example 3
[0103] A cryosleep device with high thermal insulation performance, other features are the same as those of Example 1, except that: the minimum thickness of the foam insulation layer is 10 mm.
[0104] In the foamed thermal insulation layer, by weight,
[0105] Polyether polyol: 40 parts;
[0106] 2-Fluorophenyl isocyanate: 28 parts;
[0107] Polyethylene glycol: 5 parts;
[0108] Aerogel microspheres: 12 parts;
[0109] Graphite fluoride: 2 parts;
[0110] Barium sulfate: 0.8 parts;
[0111] Hydromagnesite: 1 part;
[0112] Dimethicone oil: 8 parts;
[0113] N-bromosuccinimide: 1 part;
[0114] Isopentane: 8 parts;
[0115] Water: 3 parts;
[0116] Tris[2,4-di-tert-butylphenyl]phosphite: 0.4 parts.
[0117] The preparation method of the cryosleep device with high heat preservation performance is characterized by comprising the following steps:
[0118] S1, polyether polyol, polyethylene glycol, dimethyl silicone oil, aerogel microspheres, graphite fluoride, barium sulfate, hydromagnesite, N-bromosuccinimide, water and tris[2,4-di-tert-butylphenyl]phosphite, stirring at a stirring speed of 120 r / min for 30 min, and then entering S2;
[0119] S2, add 2-fluorophenyl isocyanate, stir at a stirring speed of 1200 r / min, stir for 30 min to obtain an intermediate, and enter S3;
[0120] S3, adding isopentane to the intermediate, stirring for 7 seconds, and then foaming to obtain a polyurethane foam semi-finished product, and then putting the polyurethane foam semi-finished product into the second structural layer 300, and the volume ratio of the intermediate to the second structural layer 300 is 1:28;
[0121] S4. The polyurethane foam semi-finished product is cured at a temperature of 115° C. for 36 hours to obtain a foamed insulation layer.
[0122] Example 4
[0123] A cryosleep device with high thermal insulation performance, such as Figure 1 As shown, other features are the same as those in Example 1, except that the minimum thickness of the foam insulation layer is 30 mm.
[0124] In the foamed thermal insulation layer, by weight,
[0125] Polyether polyol: 40 parts;
[0126] 2-Fluorophenyl isocyanate: 23 parts;
[0127] Polyethylene glycol: 7 parts;
[0128] Aerogel microspheres: 10.5 parts;
[0129] Graphite fluoride: 1.5 parts;
[0130] Barium sulfate: 0.6 parts;
[0131] Hydromagnesite: 0.7 parts;
[0132] Dimethyl silicone oil: 12 parts;
[0133] N-bromosuccinimide: 2.3 parts;
[0134] Isopentane: 9 parts;
[0135] Water: 2.5 parts;
[0136] Tris[2,4-di-tert-butylphenyl]phosphite: 0.3 parts.
[0137] The preparation method of the cryosleep device with high heat preservation performance is characterized by comprising the following steps:
[0138] S1, polyether polyol, polyethylene glycol, dimethyl silicone oil, aerogel microspheres, graphite fluoride, barium sulfate, hydromagnesite, N-bromosuccinimide, water and tris[2,4-di-tert-butylphenyl]phosphite, stirring at a stirring speed of 110 r / min for 20 min, and entering S2;
[0139] S2, add 2-fluorophenyl isocyanate, stir at a stirring speed of 1100 r / min, stir for 20 min to obtain an intermediate, and enter S3;
[0140] S3, adding isopentane to the intermediate, stirring for 8 seconds and then foaming to obtain a polyurethane foam semi-finished product, and then putting the polyurethane foam semi-finished product into the second structural layer 300, and the volume ratio of the intermediate to the second structural layer 300 is 1:26;
[0141] S4. The polyurethane foam semi-finished product is cured at a temperature of 110° C. for 24 hours to obtain a foamed insulation layer.
[0142] Example 5
[0143] A cryosleep device with high thermal insulation performance, such as Figure 1 As shown, other features are the same as those in Example 1, except that the minimum thickness of the foam insulation layer is 30 mm.
[0144] In the foamed thermal insulation layer, by weight,
[0145] Polyether polyol: 40 parts;
[0146] 2-Fluorophenyl isocyanate: 25 parts;
[0147] Polyethylene glycol: 6.5 parts;
[0148] Aerogel microspheres: 9 parts;
[0149] Graphite fluoride: 1.8 parts;
[0150] Barium sulfate: 0.7 parts;
[0151] Hydromagnesite: 0.6 parts;
[0152] Dimethyl silicone oil: 10 parts;
[0153] N-bromosuccinimide: 2 parts;
[0154] Isopentane: 9.5 parts;
[0155] Water: 1.5 parts;
[0156] Tris[2,4-di-tert-butylphenyl]phosphite: 0.25 parts.
[0157] The preparation method of the cryosleep device with high heat preservation performance is characterized by comprising the following steps:
[0158] S1, polyether polyol, polyethylene glycol, dimethyl silicone oil, aerogel microspheres, graphite fluoride, barium sulfate, hydromagnesite, N-bromosuccinimide, water and tris[2,4-di-tert-butylphenyl]phosphite, stirring at a stirring speed of 110 r / min for 20 min, and entering S2;
[0159] S2, add 2-fluorophenyl isocyanate, stir at a stirring speed of 1000 r / min, stir for 25 min to obtain an intermediate, and enter S3;
[0160] S3, adding isopentane to the intermediate, stirring for 9 seconds, and then foaming to obtain a polyurethane foam semi-finished product, and then putting the polyurethane foam semi-finished product into the second structural layer 300, and the volume ratio of the intermediate to the second structural layer 300 is 1:27;
[0161] S4. The polyurethane foam semi-finished product is cured at a temperature of 112° C. for 24 hours to obtain a foamed insulation layer.
[0162] Comparative Example 1
[0163] A cryosleep device with high thermal insulation performance, the other features are the same as those of Example 4, except that, in the foamed thermal insulation layer, by weight,
[0164] Polyether polyol: 40 parts;
[0165] 2-Fluorophenyl isocyanate: 15 parts;
[0166] Polyethylene glycol: 10 parts;
[0167] Aerogel microspheres: 5 parts;
[0168] Graphite fluoride: 0.5 part;
[0169] Barium sulfate: 1 part;
[0170] Hydromagnesite: 1.3 parts;
[0171] Dimethicone oil: 5 parts;
[0172] N-bromosuccinimide: 0.5 parts;
[0173] Isopentane: 12 parts;
[0174] Water: 0.5 parts;
[0175] Tris[2,4-di-tert-butylphenyl]phosphite: 0.1 parts.
[0176] Comparative Example 2
[0177] A cryosleep device with high thermal insulation performance, the other features are the same as those of Example 4, except that, in the foamed thermal insulation layer, by weight,
[0178] Polyether polyol: 40 parts;
[0179] 2-Fluorophenyl isocyanate: 30 parts;
[0180] Polyethylene glycol: 1 part;
[0181] Aerogel microspheres: 15 parts;
[0182] Graphite fluoride: 2.5 parts;
[0183] Barium sulfate: 0.2 parts;
[0184] Hydromagnesite: 0.3 parts;
[0185] Dimethicone oil: 18 parts;
[0186] N-bromosuccinimide: 4 parts;
[0187] Isopentane: 5 parts;
[0188] Water: 4 parts;
[0189] Tris[2,4-di-tert-butylphenyl]phosphite: 0.5 parts.
[0190] Comparative Example 3
[0191] A cryosleep device with high thermal insulation performance, the other features are the same as those of Example 4, except that no aerogel microspheres are added to the foaming insulation layer, specifically, in parts by weight,
[0192] Polyether polyol: 40 parts;
[0193] 2-Fluorophenyl isocyanate: 23 parts;
[0194] Polyethylene glycol: 7 parts;
[0195] Aerogel microspheres: 0;
[0196] Graphite fluoride: 12 parts;
[0197] Barium sulfate: 0.6 parts;
[0198] Hydromagnesite: 0.7 parts;
[0199] Dimethyl silicone oil: 12 parts;
[0200] N-bromosuccinimide: 2.3 parts;
[0201] Isopentane: 9 parts;
[0202] Water: 2.3 parts;
[0203] Tris[2,4-di-tert-butylphenyl]phosphite: 0.3 parts.
[0204] The preparation method of the cryosleep device with high heat preservation performance is characterized by comprising the following steps:
[0205] S1, polyether polyol, polyethylene glycol, dimethyl silicone oil, graphite fluoride, barium sulfate, hydromagnesite, N-bromosuccinimide, water and tris[2,4-di-tert-butylphenyl]phosphite, stirring at a stirring speed of 110 r / min for 20 min, and entering S2;
[0206] S2, add 2-fluorophenyl isocyanate, stir at a stirring speed of 1100 r / min, stir for 20 min to obtain an intermediate, and enter S3;
[0207] S3, adding isopentane to the intermediate, stirring for 8 seconds and then foaming to obtain a polyurethane foam semi-finished product, and then putting the polyurethane foam semi-finished product into the second structural layer 300, and the volume ratio of the intermediate to the second structural layer 300 is 1:26;
[0208] S4. The polyurethane foam semi-finished product is cured at a temperature of 110° C. for 24 hours to obtain a foamed insulation layer.
[0209] Comparative Example 4
[0210] A cryosleep device with high thermal insulation performance, the other features are the same as those of Example 3, except that no fluorinated graphite is added to the foamed thermal insulation layer, specifically, in parts by weight,
[0211] Polyether polyol: 40 parts;
[0212] 2-Fluorophenyl isocyanate: 23 parts;
[0213] Polyethylene glycol: 7 parts;
[0214] Aerogel microspheres: 12 parts;
[0215] Graphite fluoride: 0;
[0216] Barium sulfate: 0.6 parts;
[0217] Hydromagnesite: 0.7 parts;
[0218] Dimethyl silicone oil: 12 parts;
[0219] N-bromosuccinimide: 2.3 parts;
[0220] Isopentane: 9 parts;
[0221] Water: 2.3 parts;
[0222] Tris[2,4-di-tert-butylphenyl]phosphite: 0.3 parts.
[0223] The preparation method of the cryosleep device with high heat preservation performance is characterized by comprising the following steps:
[0224] S1, polyether polyol, polyethylene glycol, dimethyl silicone oil, aerogel microspheres, barium sulfate, hydromagnesite, N-bromosuccinimide, water and tris[2,4-di-tert-butylphenyl]phosphite, stirring at a stirring speed of 110 r / min for 20 min, and entering S2;
[0225] S2, add 2-fluorophenyl isocyanate, stir at a stirring speed of 1100 r / min, stir for 20 min to obtain an intermediate, and enter S3;
[0226] S3, adding isopentane to the intermediate, stirring for 8 seconds and then foaming to obtain a polyurethane foam semi-finished product, and then putting the polyurethane foam semi-finished product into the second structural layer 300, and the volume ratio of the intermediate to the second structural layer 300 is 1:26;
[0227] S4. The polyurethane foam semi-finished product is cured at a temperature of 110° C. for 24 hours to obtain a foamed insulation layer.
[0228] Comparative Example 5
[0229] A cryosleep device with high thermal insulation performance, the other features are the same as those of Example 3, except that barium sulfate is not added to the foam insulation layer, specifically, in parts by weight,
[0230] Polyether polyol: 40 parts;
[0231] 2-Fluorophenyl isocyanate: 23 parts;
[0232] Polyethylene glycol: 7 parts;
[0233] Aerogel microspheres: 10.5 parts;
[0234] Graphite fluoride: 1.5 parts;
[0235] Barium sulfate: 0;
[0236] Hydromagnesite: 1.3 parts;
[0237] Dimethyl silicone oil: 12 parts;
[0238] N-bromosuccinimide: 2.3 parts;
[0239] Isopentane: 9 parts;
[0240] Water: 2.3 parts;
[0241] Tris[2,4-di-tert-butylphenyl]phosphite: 0.3 parts.
[0242] The preparation method of the cryosleep device with high heat preservation performance is characterized by comprising the following steps:
[0243] S1, polyether polyol, polyethylene glycol, dimethyl silicone oil, aerogel microspheres, graphite fluoride, hydromagnesite, N-bromosuccinimide, water and tris[2,4-di-tert-butylphenyl]phosphite, stirring at a stirring speed of 110 r / min for 20 min, and entering S2;
[0244] S2, add 2-fluorophenyl isocyanate, stir at a stirring speed of 1100 r / min, stir for 20 min to obtain an intermediate, and enter S3;
[0245] S3, adding isopentane to the intermediate, stirring for 8 seconds and then foaming to obtain a polyurethane foam semi-finished product, and then putting the polyurethane foam semi-finished product into the second structural layer 300, and the volume ratio of the intermediate to the second structural layer 300 is 1:26;
[0246] S4. The polyurethane foam semi-finished product is cured at a temperature of 110° C. for 24 hours to obtain a foamed insulation layer.
[0247] Comparative Example 6
[0248] A cryosleep device with high thermal insulation performance, the other features are the same as those of Example 3, except that hydromagnesite is not added to the foamed thermal insulation layer, specifically, in parts by weight,
[0249] Polyether polyol: 40 parts;
[0250] 2-Fluorophenyl isocyanate: 23 parts;
[0251] Polyethylene glycol: 7 parts;
[0252] Aerogel microspheres: 10.5 parts;
[0253] Graphite fluoride: 1.5 parts;
[0254] Barium sulfate: 1.3 parts;
[0255] Hydromagnesite: 0;
[0256] Dimethyl silicone oil: 12 parts;
[0257] N-bromosuccinimide: 2.3 parts;
[0258] Isopentane: 9 parts;
[0259] Water: 2.3 parts;
[0260] Tris[2,4-di-tert-butylphenyl]phosphite: 0.3 parts.
[0261] The preparation method of the cryosleep device with high heat preservation performance is characterized by comprising the following steps:
[0262] S1, polyether polyol, polyethylene glycol, dimethyl silicone oil, aerogel microspheres, graphite fluoride, barium sulfate, N-bromosuccinimide, water and tris[2,4-di-tert-butylphenyl]phosphite, stirring at a stirring speed of 110 r / min for 20 min, and entering S2;
[0263] S2, add 2-fluorophenyl isocyanate, stir at a stirring speed of 1100 r / min, stir for 20 min to obtain an intermediate, and enter S3;
[0264] S3, adding isopentane to the intermediate, stirring for 8 seconds and then foaming to obtain a polyurethane foam semi-finished product, and then putting the polyurethane foam semi-finished product into the second structural layer 300, and the volume ratio of the intermediate to the second structural layer 300 is 1:26;
[0265] S4. The polyurethane foam semi-finished product is cured at a temperature of 110° C. for 24 hours to obtain a foamed insulation layer.
[0266] Comparative Example 7
[0267] A cryosleep device with high thermal insulation performance, the other features of which are the same as those of Example 4, except that in the foaming insulation layer, 2-fluorophenyl isocyanate is replaced with isocyanate.
[0268] Effect example
[0269] The foamed thermal insulation layer obtained in Examples 2 to 5 of the present invention and the foamed thermal insulation layer obtained in Comparative Examples 1 to 7 were subjected to performance tests, wherein the thermal conductivity was tested according to the standard GB / T10295-2008, the tensile strength at -170°C was tested according to 1SO1926, the average pore diameter was tested according to GB / T 8810-2005, and the closed cell rate was tested according to ASTMD2856-94. The test results are shown in Tables 1 and 2:
[0270] Table 1. Test results of foam insulation layer performance of Examples 2-5
[0271]
[0272] Table 2. Test results of foam insulation layer of comparative examples 1-7
[0273]
[0274]
[0275] It can be seen from the data in Table 1 and Table 2 that, compared with the foam insulation layer of the comparative example, the thermal conductivity of the foam insulation layer of Examples 2-5 of the present invention is significantly smaller than that of Comparative Examples 1-8, and within the range of 0.0171W / m·K to 0.0192W / m·K, the closed cell rate is not less than 96.15%, so the thermal insulation performance of the present invention is excellent. The tensile strength of the foam insulation layer of the present invention can still maintain a relatively high strength at -170°C, so it has high tensile strength and good mechanical properties. By filling the foam insulation layer between the accommodating liner 400 and the double-layer insulation structure, support can be provided for the accommodating liner 400. Moreover, the foam core density of the foam insulation layer of the present invention is 0.226g / cm 3 ~0.243g / cm 3 , and its weight is small. It can be seen from the foaming density and average cell diameter of the present invention that the foaming insulation layer of the present invention has more cell data and a small cell diameter.
[0276] The cryosleep device with high thermal insulation performance of the present invention can effectively block the conduction of ambient heat to the cryosleep liquid through double thermal insulation of the vacuum interlayer and the foamed thermal insulation layer, thereby preventing the outer wall of the cryosleep device from freezing to the operator, and can also reduce refrigeration energy consumption, thereby achieving energy conservation and emission reduction.
[0277] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A cryosleep device with high heat preservation performance, characterized in that: A main body and a container for containing a cryosleep liquid are provided, the container is assembled inside the main body, a double-layer insulation structure is provided outside the container, the double-layer insulation structure is provided with a first structure layer and a second structure layer, the first structure layer is close to the container, the second structure layer is located outside the first structure layer, the first structure layer is a vacuum interlayer, and a foam insulation layer is filled in the second structure layer; The raw materials of the foaming insulation layer contain polyether polyol, 2-fluorophenyl isocyanate, polyethylene glycol, aerogel microspheres, barium sulfate, fluorinated graphite and hydromagnesite, dimethyl silicone oil, N-bromosuccinimide, isopentane, water and tris[2.4-di-tert-butylphenyl]phosphite.
2. The cryosleep device with high heat preservation performance according to claim 1, characterized in that: The thermal conductivity of the foamed insulation layer is 0.0171W / m·K to 0.0192W / m·K.
3. The cryosleep device with high heat preservation performance according to claim 1, characterized in that: The closed cell rate of the foamed heat-insulating layer is 96.15% to 96.99%.
4. The cryosleep device with high heat preservation performance according to claim 1, characterized in that: The average diameter of the pores in the foamed thermal insulation layer is 0.182 mm to 0.186 mm.
5. The cryosleep device with high heat preservation performance according to claim 1, characterized in that: The foam core density of the foam insulation layer is 0.226 g / cm 3 ~0.243g / cm 3 .
6. The cryosleep device with high heat preservation performance according to claim 1, characterized in that: The minimum thickness of the foam insulation layer is 10 mm to 30 mm.
7. The cryosleep device with high heat preservation performance according to claim 1, characterized in that: In the foamed thermal insulation layer, by weight, Polyether polyol: 40 parts; 2-Fluorophenyl isocyanate: 18 to 28 parts; Polyethylene glycol: 3 to 8 parts; Aerogel microspheres: 8 to 12 parts; Graphite fluoride: 1 to 2 parts; Barium sulfate: 0.4 to 0.8 parts; Hydromagnesite: 0.5 to 1 part; Dimethyl silicone oil: 8 to 15 parts; N-bromosuccinimide: 1 to 3 parts; Isopentane: 8 to 10 parts; Water: 1 to 3 parts; Tris[2,4-di-tert-butylphenyl]phosphite: 0.2 to 0.4 parts.
8. The cryosleep device with high heat preservation performance according to claim 7, characterized in that: In the foamed thermal insulation layer, by weight, In the foamed thermal insulation layer, by weight, Polyether polyol: 40 parts; 2-Fluorophenyl isocyanate: 23 parts; Polyethylene glycol: 7 parts; Aerogel microspheres: 10.5 parts; Graphite fluoride: 1.5 parts; Barium sulfate: 0.6 parts; Hydromagnesite: 0.7 parts; Dimethyl silicone oil: 12 parts; N-bromosuccinimide: 2.3 parts; Isopentane: 9 parts; Water: 2.5 parts; Tris[2,4-di-tert-butylphenyl]phosphite: 0.3 parts.
9. The cryosleep device with high heat preservation performance according to claim 1, characterized in that: The method for preparing the foamed thermal insulation layer comprises the following steps: S1, mixing polyether polyol, polyethylene glycol, dimethyl silicone oil, aerogel microspheres, graphite fluoride, barium sulfate, hydromagnesite, N-bromosuccinimide, water and tris[2,4-di-tert-butylphenyl]phosphite, and entering S2; S2, add 2-fluorophenyl isocyanate, stir and mix to obtain an intermediate, and proceed to S3; S3, adding isopentane to the intermediate to foam it to obtain a polyurethane foam semi-finished product, and then injecting the polyurethane foam semi-finished product into the second structural layer; S4, ripening the accommodating liner, the double-layer insulation structure and the polyurethane foam semi-finished product as a whole to obtain the foam insulation layer.
10. The cryosleep device with high heat preservation performance according to claim 9, characterized in that: The method for preparing the foamed thermal insulation layer comprises the following steps: S1, polyether polyol, polyethylene glycol, dimethyl silicone oil, aerogel microspheres, graphite fluoride, barium sulfate, hydromagnesite, N-bromosuccinimide, water and tris[2,4-di-tert-butylphenyl]phosphite, stirring at a stirring speed of 100 r / min to 120 r / min for 15 min to 30 min, and then entering S2; S2, add 2-fluorophenyl isocyanate, stir at a stirring speed of 1000 r / min to 1200 r / min, stir for 15 min to 30 min to obtain an intermediate, and enter S3; S3, adding isopentane to the intermediate, stirring for 7s to 10s and then foaming to obtain a polyurethane foam semi-finished product, and then adding the polyurethane foam semi-finished product into the second structural layer, and the volume ratio of the intermediate to the second structural layer is 1:25 to 28; S4. Curing the accommodating liner, the double-layer insulation structure and the polyurethane foam semi-finished product as a whole at a curing temperature of 105° C. to 115° C. for a curing time of 18 h to 36 h to obtain the foam insulation layer.