Method for evaluating hydrogen resistance of metal material
By conducting detailed evaluation of hydrogen concentration and stress loading on high-strength steel, the minimum pressure-break stress and threshold hydrogen concentration are determined, which solves the problem of difficult to evaluate the risk of hydrogen embrittlement in the existing technology, and realizes the quantification of the hydrogen resistance performance of metal materials Assessment and risk reduction.
Patent Information
- Application Number
- CN202310554151.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-17
- Publication Date
- 2024-11-22
AI Technical Summary
The prior art lacks unified standards and refinement methods to quantify the impact of hydrogen content and stress on hydrogen embrittlement properties in high-strength steels, making it difficult to evaluate and control the risk of hydrogen embrittlement.
By preparing samples with different hydrogen concentrations, tensile strength measurement, thermal desorption and hydrogen removal, electrochemical hydrogen charging and bending tests, a hydrogen concentration change curve was established, and combined with stress loading, the minimum pressure-breaking stress and threshold hydrogen concentration of metal materials were determined. , to evaluate its hydrogen resistance.
A quantitative assessment of the risk of hydrogen embrittlement of metal materials has been achieved, providing a scientific basis for guiding its use and improvement, and reducing the risk of hydrogen embrittlement.
Smart Images

Figure BDA0004232372790000081 
Figure BDA0004232372790000101 
Figure BDA0004232372790000111
Abstract
Description
Technical Field
[0001] The invention relates to the field of hydrogen embrittlement of metal materials, and in particular to a method for evaluating the hydrogen resistance of metal materials, which is mainly used for hydrogen resistance testing of high-strength automobile steel. Background Art
[0002] Hydrogen embrittlement is one of the important ways in which metal materials fail. Hydrogen embrittlement has the following significant characteristics: (1) deterioration of mechanical properties, especially significant reduction of elongation and cross-sectional shrinkage; (2) change of fracture mechanism, forming different fracture morphologies, mainly manifested in that as the hydrogen concentration in the material increases, the fracture mode changes from ductile dimple fracture to brittle cleavage or intergranular fracture; (3) fracture occurs suddenly without obvious signs, which often leads to serious consequences. Hydrogen embrittlement may occur in metal materials during production, processing and use. Among them, diffuse hydrogen is one of the key factors leading to hydrogen embrittlement of metals. The higher the concentration of diffuse hydrogen in the metal matrix, the greater the risk of hydrogen embrittlement of the metal material.
[0003] In recent years, with the development of lightweight automobile industry, high-strength automobile steel has been widely used, the strength of high-strength steel has been getting higher and higher, and the risk of hydrogen embrittlement has been getting higher and higher. Using effective hydrogen embrittlement evaluation methods to evaluate the hydrogen resistance of metal materials, especially high-strength steel metal materials, is conducive to reducing the risks in the use of high-strength steel.
[0004] At present, there is no unified standard for the hydrogen embrittlement evaluation test of high-strength steel in China. At present, the standards adopted by major domestic OEMs include Mazda's "HYDROGEN EMBRITTLEMENT EVAL." material testing standard, which mainly evaluates high-strength steel plates and high-strength steel welding parts. After electrodeposition of U-shaped and V-shaped samples, observe whether cracks occur, and then test the diffusible hydrogen content of the samples by TDA method. General Motors' "SEP 1970 Hydrogen Cracking Test" standard, which mainly processes the sample into a U-shaped sample and places it for 720 hours, then observes whether cracks occur; at the same time, a perforated tensile sample is made for stretching, and the tensile force is the yield strength. After 96 hours of stretching, observe whether the sample breaks. Tesla's "TM-2011 Rev 06 Steel, Rolled Product-Sheet and Strip" standard requires that according to Tesla's material requirements, high-strength steel needs to pass a 300-hour hydrochloric acid immersion test. Nissan's "HCl Test Procedure for U-bend test samples for Nissan Approval" standard mainly applies different stress levels to high-strength steel and then immerses it in hydrochloric acid solution for 300-1000 hours to observe whether there are cracks on the surface of the high-strength steel.
[0005] The above existing standards use whether the sample cracks as the delayed cracking evaluation index, which is relatively superficial. The delayed cracking of the sample is mainly caused by the combined effects of materials, stress and hydrogen introduced by environmental corrosion. Since the structure and properties of a given material are constant, the main factor causing delayed cracking depends on the hydrogen introduced by stress and environmental corrosion. In the process of evaluating delayed cracking of materials, the existing standards cannot quantify the relationship between stress, hydrogen content and delayed cracking of materials; and the hydrogen introduced into the sample mostly exists in reversible hydrogen traps in the material such as grain boundaries, dislocations, inclusions and vacancies. Therefore, if the relationship between hydrogen content and material hydrogen resistance can be clarified, the influence of material structure defects on material hydrogen resistance can also be clarified, thereby providing support for improving material hydrogen resistance from a mechanism perspective.
[0006] The present invention combines stress with hydrogen content to evaluate the hydrogen resistance of materials, and can quantify the relationship between stress, hydrogen content and the hydrogen resistance of materials. It is more detailed and in-depth than traditional standards, and also provides support for material research and development and improvement. Summary of the invention
[0007] In view of the defects existing in the prior art, the purpose of the present invention is to provide a method for evaluating the hydrogen resistance of metal materials. For a given metal material, by loading different stresses under different hydrogen concentrations, the hydrogen concentration and minimum fracture stress at which the metal material does not suffer from hydrogen embrittlement are obtained, thereby providing guidance for the hydrogen embrittlement risk of the metal material and timely reducing the risk of using the metal material.
[0008] In order to achieve the above object, the present invention adopts the following technical solution:
[0009] The present invention provides a method for evaluating the hydrogen resistance of a metal material, comprising the following steps:
[0010] S1, preparing a metal material into a sample, and removing free hydrogen in the sample by heating;
[0011] S2, tensile strength measurement, determining the tensile strength of the sample by a slow tensile test;
[0012] S3, removing hydrogen by thermal desorption, removing diffusible hydrogen in the sample by thermal desorption;
[0013] S4, electrochemical hydrogen charging, using the electrochemical method to place the dehydrogenated sample in a hydrogen charging solution for different lengths of time;
[0014] S5, measuring the saturated hydrogen concentration, measuring the hydrogen of the samples obtained in step S4 one by one according to the hydrogen charging time, determining the saturated hydrogen concentration of the samples by comparison, and establishing a hydrogen charging concentration change curve;
[0015] S6, according to the hydrogen charging concentration change curve obtained in step S5, a plurality of hydrogen-charged samples with different hydrogen concentrations are prepared, and bending tests with different stresses are performed respectively to obtain the minimum compressive stress of the hydrogen-charged samples with each hydrogen concentration, and the hydrogen resistance of the metal material is judged accordingly.
[0016] Preferably, in step S1:
[0017] The sample is surface treated with acetone ultrasound for a treatment time of >15 min; and / or
[0018] During the heating process, the heating temperature is 150-200° C. and the heating time is 15-120 min; and / or
[0019] After the heat treatment, the free hydrogen concentration in the sample was reduced to below 0.02 ppm.
[0020] Preferably, in step S3, during the thermal desorption process for removing hydrogen, the sample is heated to 400° C. and maintained at that temperature for 20 to 60 minutes.
[0021] Preferably, in step S4:
[0022] The hydrogen charging solution is 0.5 mol / L H2SO4+0.3 g / L thiourea solution; and / or
[0023] The hydrogen charging current during the electrochemical hydrogen charging process is 10 mA / cm 2 and / or
[0024] The hydrogen charging times of different lengths are 10 to 600 minutes.
[0025] Preferably, in step S5, during the saturated hydrogen concentration determination process, the difference between the hydrogen contents of samples with different hydrogen filling times is compared until the difference between the hydrogen contents of samples with different hydrogen filling times is less than 0.1 ppm, and the hydrogen content at this time is the saturated hydrogen concentration of the sample.
[0026] Preferably, in step S6:
[0027] The hydrogen concentration of the hydrogen-filled samples with different hydrogen concentrations is 0.02 to 0.8 times the saturated hydrogen concentration; and / or
[0028] During the bending test, the hydrogen-filled sample is loaded with different stresses, the radius of the loading pressure head is 4 to 5 times the sample thickness, and the loading time is controlled within 20 minutes.
[0029] Preferably, in step S6, during the bending test, if the hydrogen-charged sample does not crack after the initial stress loading is performed on the hydrogen-charged sample, the stress is sequentially increased from 0.4 times the tensile strength until the hydrogen-charged sample cracks, and the stress at this time is the minimum compressive stress of the hydrogen-charged sample.
[0030] Preferably, in step S6, the calculation formula of the initial stress of the bending test is as follows:
[0031] K 初 =(1.2-C H / C m )×K;
[0032] Among them, K 初 is the initial stress, in MPa;
[0033] C H is the hydrogen concentration of the hydrogen-filled sample, in ppm;
[0034] C m is the saturated hydrogen concentration of the sample, in ppm;
[0035] K is the reference stress, in MPa.
[0036] Preferably, in step S6, the reference stress is determined by the following steps:
[0037] Electrochemically charging the sample after dehydrogenation treatment according to the hydrogen charging concentration variation curve to charge the sample to a saturated hydrogen concentration, thereby obtaining a saturated hydrogen concentration sample;
[0038] The saturated hydrogen concentration sample is subjected to a bending test, and different stresses are loaded on the saturated hydrogen concentration sample. The stress loading time is controlled within 20 minutes, and the loading stress is increased from 0.2 times the tensile strength to 0.3 to 1.0 times the tensile strength in sequence until the saturated hydrogen concentration sample breaks. The stress when the saturated hydrogen concentration sample breaks is recorded as the reference stress K.
[0039] Preferably, in step S6, the hydrogen resistance of the metal material is determined by the following method:
[0040] The ratio of the minimum compressive stress to the tensile strength of the hydrogen-charged sample is calculated. When the ratio is ≥0.8, the hydrogen-charged sample has qualified hydrogen resistance. At this time, the hydrogen concentration corresponding to the hydrogen-charged sample with qualified hydrogen resistance is the threshold hydrogen concentration of the metal material.
[0041] The principle of the method for evaluating the hydrogen resistance of metal materials of the present invention is as follows: hydrogen embrittlement of metal materials is mainly caused by the combined effects of the material structure itself, the concentration of diffused hydrogen inside the metal material and the stress. For the same metal material, hydrogen embrittlement will not occur under lower hydrogen concentrations and lower stresses. Based on this, for a given metal material, under different hydrogen concentrations, by loading different stresses, the hydrogen concentration and stress at which the metal material does not undergo hydrogen embrittlement, i.e., the threshold hydrogen concentration and threshold stress, can be obtained, which can be used as the hydrogen resistance index of the metal material.
[0042] The method for evaluating the hydrogen resistance of metal materials of the present invention has the following beneficial effects:
[0043] 1. The method for evaluating the hydrogen resistance of metal materials of the present invention can obtain the threshold hydrogen concentration of high-strength steels with different strengths and the minimum stress under different hydrogen concentration conditions, and can quantify the hydrogen embrittlement risk to a certain extent through the relationship between hydrogen concentration and stress, and more directly clarify the hydrogen resistance of the material;
[0044] 2. The stress-hydrogen concentration relationship curve obtained by the method for evaluating the hydrogen resistance of metal materials of the present invention can be used to guide the use of metal materials. At the same time, it can also evaluate the hydrogen embrittlement risk of metal materials during actual use, and take timely measures to reduce the risk of metal material use;
[0045] 3. The method for evaluating the hydrogen resistance of metal materials of the present invention can obtain the risk of hydrogen embrittlement and cracking of metal materials under different hydrogen concentrations and stress conditions, and provide preventive measures for hydrogen embrittlement of metal materials. In addition, the method of the present invention can be combined with changes in alloy content, production process changes and other factors to evaluate the influence of various factors on the hydrogen resistance of metal materials, and provide guidance for reducing the risk of hydrogen embrittlement of metal materials. DETAILED DESCRIPTION
[0046] The present invention will be described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form.
[0047] The method for evaluating the hydrogen resistance of a metal material provided by the present invention comprises the following steps:
[0048] S1, preparing a metal material into a sample and removing free hydrogen in the sample by heating;
[0049] Specifically, the metal material was sheared into samples of 120 mm*20 mm in size to ensure that the sample surface was flat and without bending, with 20 samples of each type. The sample was surface treated with acetone ultrasound for a treatment time of >15 min to ensure that the sample surface was clean.
[0050] The sample is heated in a heating furnace to remove free hydrogen in the sample, wherein the heating temperature is 150-200° C. and the heating time is 15-120 min (in a further preferred embodiment, the heating time is 20-60 min), so that the free hydrogen concentration in the sample is reduced to below 0.02 ppm.
[0051] S2, tensile strength measurement, the tensile strength of the sample is determined by a slow tensile test;
[0052] Specifically, using a slow tensile testing machine, select 3 samples for slow tensile testing to obtain a slow tensile curve, and determine the tensile strength of the 3 samples based on the slow tensile curve. To ensure data accuracy, the difference in the tensile strength of the 3 samples must be less than 100 MPa, and the average tensile strength of the 3 samples is taken as the tensile strength of the test material.
[0053] S3, thermal desorption method to remove hydrogen, thermal desorption method is used to remove the diffusible hydrogen in the sample;
[0054] Specifically, a German Bruker hydrogen analyzer was used to heat the sample to 400°C using a thermal desorption method, and the temperature was maintained for 20 to 60 minutes to remove the diffusible hydrogen in the sample, and the diffusible hydrogen content was obtained to determine that the hydrogen content in the sample was less than 0.02 ppm.
[0055] S4, electrochemical hydrogen charging, using the electrochemical method to place the dehydrogenated sample in a hydrogen charging solution for different lengths of time;
[0056] Specifically, 0.5 mol / L H2SO4+0.3 g / L thiourea solution was prepared as the hydrogen charging solution and stored at room temperature for 24 h before use; then, a constant current mode was used with a current of 10 mA / cm 2 The constant current is used as the hydrogen charging current, and the sample after the dehydrogenation treatment is placed in the hydrogen charging solution for hydrogen charging for different lengths of time. The hydrogen charging time varies from 10 to 600 minutes. In a specific embodiment, the hydrogen charging time can be 10 to 300 minutes. Thereafter, the samples charged with hydrogen for different lengths of time are placed in liquid nitrogen for storage for later use.
[0057] S5, measuring the saturated hydrogen concentration, measuring the hydrogen of the samples obtained in step S4 one by one according to the hydrogen charging time, determining the saturated hydrogen concentration of the samples by comparison, and establishing a hydrogen charging concentration change curve;
[0058] Specifically, the samples charged with hydrogen for different lengths of time are measured one by one according to the charging time, and the difference in hydrogen content between the samples with different charging time is compared until the difference in hydrogen content between the samples with different charging time is less than 0.1ppm. The hydrogen content at this time is the saturated hydrogen concentration of the sample. At the same time, the relationship between the hydrogen charging concentration and time is recorded to establish a hydrogen charging concentration change curve.
[0059] S6. According to the hydrogen charging concentration variation curve obtained in step S5, the sample after dehydrogenation in step S3 is once again charged with hydrogen to prepare a plurality of hydrogen charged samples with different hydrogen concentrations. The hydrogen charged samples with different hydrogen concentrations are subjected to bending loading tests with different stresses, so as to obtain the minimum compressive stress corresponding to the hydrogen charged sample with each hydrogen concentration, and judge the hydrogen resistance of the metal material based on the stress.
[0060] Specifically, first, according to the hydrogen charging concentration change curve obtained in step S5, the sample after dehydrogenation in step S3 is once again charged with hydrogen, and multiple hydrogen charging samples with different hydrogen concentrations (the hydrogen concentration range is 0.02 to 0.8 times the saturated hydrogen concentration) are prepared and placed in a liquid nitrogen tank for standby. Hydrogen charging samples with different hydrogen concentrations are selected, and after thawing, a bending test is performed using a U bending tester, and different stresses are applied to the hydrogen charging samples with different hydrogen concentrations; wherein, the radius of the loading head is 4 to 5 times the sample thickness, and the loading time is controlled within 20 minutes (for example, 5 minutes).
[0061] When loading different stresses on a hydrogen-charged sample of a certain hydrogen concentration, firstly perform an initial stress loading on the hydrogen-charged sample. If the hydrogen-charged sample does not crack, then increase the stress successively from 0.4 times the tensile strength until the hydrogen-charged sample cracks. The stress at this time is the minimum compressive stress of the hydrogen-charged sample. Then, the hydrogen resistance of the metal material is judged according to the minimum compressive stress of the hydrogen-charged sample and the tensile strength of the sample. Specifically, the judgment is made by the following method: the ratio of the minimum compressive stress to the tensile strength of the hydrogen-charged sample is calculated. When the ratio is ≥0.8, the hydrogen resistance of the hydrogen-charged sample is qualified. At this time, the hydrogen concentration corresponding to the hydrogen-charged sample is regarded as the threshold hydrogen concentration of the metal material.
[0062] When conducting a bending test on a metal material, since its minimum compressive stress is unknown, a certain minimum stress (i.e., initial stress) is first used for loading to quickly determine the minimum compressive stress reference range, thereby shortening the test time. The initial stress is only used as the basis for further judging the minimum fracture stress. If cracks appear in the metal material sample during the initial stress loading, it can be seen that the metal material has extremely poor hydrogen resistance. At this time, the test should be terminated without further testing the hydrogen resistance of the metal material.
[0063] In the bending test process described above, the initial stress is calculated by the following formula: K 初 =(1.2-C H / C m )×K; where K 初 is the initial stress, in MPa; C H is the hydrogen concentration of the hydrogen-filled sample, in ppm; C m is the saturated hydrogen concentration of the sample, in ppm; K is the reference stress, in MPa.
[0064] The reference stress is determined by the following steps:
[0065] Preparation of saturated hydrogen concentration samples: First, the sample after dehydrogenation treatment is electrochemically charged with hydrogen according to the hydrogen charging concentration change curve, and hydrogen is charged to the saturated hydrogen concentration to obtain 4 saturated hydrogen concentration samples, which are placed in a liquid nitrogen tank for standby use.
[0066] Determine the radius of the loading head: measure the sample thickness T, set the radius R of the loading head to 4 to 5 times the sample thickness T, and round up;
[0067] Determination of reference stress: After thawing the saturated hydrogen concentration sample, it is loaded using a U bending tester. Different stresses are applied by the loading pressure head. To prevent the test distortion caused by hydrogen escape in the saturated hydrogen concentration sample, the loading time needs to be controlled within 20 minutes. The loading stress starts from 0.2 times the tensile strength and is gradually increased to 0.3 to 1.0 times the tensile strength until the saturated hydrogen concentration sample cracks. The stress at this time is recorded as the reference stress K.
[0068] The method for evaluating the hydrogen resistance of a metal material of the present invention is further described below with reference to specific examples;
[0069] Example 1
[0070] In this embodiment, DP1180 cold-rolled finished plate is selected from the production site as the test material, and the specific steps are as follows:
[0071] (1) Sample preparation: Cut the samples into a size of 120 mm*20 mm by shearing, ensuring that the sample surface is flat and without bending, 20 pieces of each sample;
[0072] (2) Sample surface treatment: The sample was ultrasonicated for 15 min using acetone ultrasonic method to ensure the sample surface was clean;
[0073] (3) Removal of free hydrogen in the sample: The sample was heated at 170°C in a heating furnace for 25 min to ensure that the free hydrogen concentration in the sample was reduced to below 0.02 ppm;
[0074] (4) Tensile strength (TS) measurement: Using a slow tensile testing machine, three samples were selected for slow tensile testing. The tensile strengths of the three groups of samples were 1195 MPa / 1140 MPa / 1221 MPa, respectively. The average value of 1185 MPa was taken as the tensile strength of the sample.
[0075] (5) Hydrogen removal by thermal desorption: Using a German Bruker hydrogen analyzer, the sample was heated at 400°C for 30 min to remove the diffusible hydrogen in the sample and obtain the diffusible hydrogen content of the sample;
[0076] (6) preparing a hydrogen charging solution: preparing a 0.5 mol / L H2SO4+0.3 g / L thiourea solution as a hydrogen charging solution and storing it at room temperature for 24 h for later use;
[0077] (7) Electrochemical hydrogen charging: using electrochemical constant current mode with 10mA / cm 2 The samples after dehydrogenation treatment are placed in hydrogen charging solution for hydrogen charging for different lengths of time with large and small hydrogen charging currents, ranging from 30min to 5h. The specific hydrogen charging time is 30min / 1h / 2h / 4h / 5h respectively.
[0078] (8) Sample storage: The hydrogen-filled samples are placed in liquid nitrogen for future use;
[0079] (9) Saturated hydrogen concentration and hydrogen concentration change curve: The hydrogen-filled samples are measured one by one according to the hydrogen filling time until the difference between the hydrogen contents is less than 0.1 ppm, and the sample saturated hydrogen concentration is obtained to be 3 ppm. At the same time, the relationship between the hydrogen filling concentration and time is recorded to establish a hydrogen concentration change curve;
[0080] (10) Saturated hydrogen concentration (C m ) Sample preparation: Using the hydrogen concentration change curve, the sample is electrochemically charged with hydrogen until the hydrogen concentration is saturated, and 4 pieces of saturated hydrogen concentration samples are obtained and placed in a liquid nitrogen tank for standby use;
[0081] (11) Loading head radius: The sample thickness is 1.4 mm, and the radius R is set to 6 mm;
[0082] (12) Determination of reference stress: After thawing, the saturated hydrogen concentration sample was loaded using a U-bending test machine. The loading head was selected by calculation to load different stresses. The loading time was 5 min. The loading stress started from 0.2 times the tensile strength, i.e., 237 MPa. The stress was gradually increased until the saturated hydrogen concentration sample cracked. The stress at this time was the reference stress of 590 MPa.
[0083] (13) Preparation of hydrogen charging samples: Prepare hydrogen charging samples with hydrogen concentrations of 0.15 ppm, 0.3 ppm, 0.6 ppm, and 1.2 ppm using the hydrogen concentration curve and place them in a liquid nitrogen tank for standby use;
[0084] (14) Test stress of hydrogen-filled samples: Based on the initial stress, the formula K 初 =(1.2-C H / C m )×K, the initial stresses of several groups of samples were 680MPa, 650MPa, 590MPa, and 475MPa respectively;
[0085] (15) Threshold hydrogen concentration measurement and hydrogen resistance performance determination: Using a U-bend test machine, samples with different hydrogen concentrations were selected for bending tests. The initial stress of the test was determined by the formula in step 14. The test stress head selection and steps were carried out with reference to steps 11 and 12. The four groups of hydrogen-charged samples did not break after loading the initial stress. The stress was then increased from 0.4 times the tensile strength until the hydrogen-charged samples cracked. The test results are shown in Table 1. It can be seen that under the condition of a hydrogen concentration of 0.15 ppm, the minimum breaking stress reached 1032 MPa, reaching 0.87 times the tensile strength. The ratio of the minimum breaking stress to the tensile strength exceeded 0.8. The hydrogen-charged samples with this hydrogen concentration met the requirements, while the other hydrogen-charged samples did not meet the requirements. Thus, the threshold hydrogen concentration of DP1180 cold-rolled sheet was obtained to be 0.15 ppm.
[0086] Table 1
[0087]
[0088] Example 2
[0089] In this embodiment, QP1180 cold-rolled finished plate is selected from the production site as the test material, and the specific steps are as follows:
[0090] (1) Sample preparation: Cut the samples into a size of 120 mm*20 mm by shearing, ensuring that the sample surface is flat and without bending, 20 pieces of each sample;
[0091] (2) Sample surface treatment: The sample was ultrasonicated for 15 min using acetone ultrasonic method to ensure the sample surface was clean;
[0092] (3) Removal of free hydrogen in the sample: The sample was heated at 160°C in a heating furnace for 28 min to ensure that the free hydrogen concentration in the sample was reduced to below 0.02 ppm;
[0093] (4) Tensile strength (TS) measurement: Using a slow tensile testing machine, three samples were selected for slow tensile testing. The tensile strengths of the three groups of samples were 1188 MPa / 1230 MPa / 1175 MPa, respectively. The average value of 1197 MPa was taken as the tensile strength of the sample.
[0094] (5) Hydrogen removal by thermal desorption: Using a German Bruker hydrogen analyzer, the sample was heated at 400°C for 25 min to remove the diffusible hydrogen in the sample and obtain the diffusible hydrogen content of the sample;
[0095] (6) preparing a hydrogen charging solution: preparing a 0.5 mol / L H2SO4+0.3 g / L thiourea solution as a hydrogen charging solution and storing it at room temperature for 24 h for later use;
[0096] (7) Electrochemical hydrogen charging: using electrochemical constant current mode with 10mA / cm 2 The samples after dehydrogenation treatment were placed in hydrogen charging solution for different lengths of hydrogen charging with large and small hydrogen charging currents. The hydrogen charging time ranged from 10min to 5h, and the specific hydrogen charging time was 10min / 0.5h / 1h / 3h / 5h respectively.
[0097] (8) Sample storage: The hydrogen-filled samples are placed in liquid nitrogen for future use;
[0098] (9) Saturated hydrogen concentration and hydrogen concentration change curve: The hydrogen-filled samples are measured one by one according to the hydrogen filling time until the difference between the hydrogen contents is less than 0.1 ppm, and the sample saturated hydrogen concentration is obtained to be 3.5 ppm. At the same time, the relationship between the hydrogen filling concentration and time is recorded to establish a hydrogen concentration change curve;
[0099] (10) Saturated hydrogen concentration (C m ) Sample preparation: Using the hydrogen concentration change curve, the sample is electrochemically charged with hydrogen until the hydrogen concentration is saturated, and 4 pieces of saturated hydrogen concentration samples are obtained and placed in a liquid nitrogen tank for standby use;
[0100] (11) Loading head radius: The sample thickness is 1.2 mm, and the radius R is set to 6 mm;
[0101] (12) Determination of reference stress: After thawing, the saturated hydrogen concentration sample was loaded using a U-bending test machine. The loading head was selected by calculation to load different stresses. The loading time was 5 min. The loading stress started from 0.2 times the tensile strength, i.e., 240 MPa. The stress was gradually increased until the saturated hydrogen concentration sample cracked. The stress at this time was the reference stress of 480 MPa.
[0102] (13) Preparation of hydrogen charging samples: using the hydrogen concentration curve, prepare hydrogen charging samples with hydrogen concentrations of 0.18 ppm, 0.35 ppm, 0.7 ppm, and 1.4 ppm, and place them in a liquid nitrogen tank for standby use;
[0103] (14) Test stress of hydrogen-filled samples: Based on the initial stress, the formula K 初 =(1.2-C H / C m )×K, the initial stresses of several groups of samples were 550MPa, 530MPa, 480MPa, and 380MPa respectively;
[0104] (15) Threshold hydrogen concentration measurement and hydrogen resistance performance determination: Using a U-bend test machine, samples with different hydrogen concentrations were selected for bending tests. The initial stress of the test was determined by the formula in step 14. The test stress head selection and steps were carried out with reference to steps 11 and 12. The four groups of hydrogen-charged samples did not break after loading the initial stress. The stress was then increased from 0.4 times the tensile strength until the hydrogen-charged samples cracked. The test results are shown in Table 2. It can be seen that under the condition of a hydrogen concentration of 0.18 ppm, the minimum compressive stress reached 990 MPa, reaching 0.83 times the tensile strength. The ratio of the minimum compressive stress to the tensile strength exceeded 0.8. The hydrogen-charged samples with this hydrogen concentration met the requirements, while the other hydrogen-charged samples did not meet the requirements. Thus, the threshold hydrogen concentration of QP1180 cold-rolled sheet was 0.18 ppm.
[0105] Table 2
[0106]
[0107] Example 3
[0108] In this embodiment, MS1300 cold-rolled finished plate is selected from the production site as the test material, and the specific steps are as follows:
[0109] (1) Sample preparation: Cut the samples into a size of 120 mm*20 mm by shearing, ensuring that the sample surface is flat and without bending, 20 pieces of each sample;
[0110] (2) Sample surface treatment: The sample was ultrasonicated for 15 min using acetone ultrasonic method to ensure the sample surface was clean;
[0111] (3) Removal of free hydrogen in the sample: The sample was heated at 170°C in a heating furnace for 20 min to ensure that the free hydrogen concentration in the sample was reduced to below 0.02 ppm;
[0112] (4) Tensile strength (TS) measurement: Using a slow tensile testing machine, three samples were selected for slow tensile testing. The tensile strengths of the three groups of samples were 1386 MPa / 1330 MPa / 1364 MPa, respectively. The average value of 1360 MPa was taken as the tensile strength of the sample;
[0113] (5) Hydrogen removal by thermal desorption: Using a German Bruker hydrogen analyzer, the sample was heated at 400°C for 25 min to remove the diffusible hydrogen in the sample and obtain the diffusible hydrogen content of the sample;
[0114] (6) preparing a hydrogen charging solution: preparing a 0.5 mol / L H2SO4+0.3 g / L thiourea solution as a hydrogen charging solution and storing it at room temperature for 24 h for later use;
[0115] (7) Electrochemical hydrogen charging: using electrochemical constant current mode with 10mA / cm2 The samples after dehydrogenation treatment were placed in hydrogen charging solution for different lengths of hydrogen charging with large and small hydrogen charging currents. The hydrogen charging time ranged from 10min to 5h, and the specific hydrogen charging time was 10min / 0.5h / 1h / 3h / 5h respectively.
[0116] (8) Sample storage: The hydrogen-filled samples are placed in liquid nitrogen for future use;
[0117] (9) Saturated hydrogen concentration and hydrogen concentration change curve: The hydrogen-filled samples are measured one by one according to the hydrogen filling time until the difference between the hydrogen contents is less than 0.1 ppm, and the sample saturated hydrogen concentration is obtained to be 1 ppm. At the same time, the relationship between the hydrogen filling concentration and time is recorded to establish a hydrogen concentration change curve;
[0118] (10) Saturated hydrogen concentration (C m ) Sample preparation: Using the hydrogen concentration change curve, the sample is electrochemically charged with hydrogen until the hydrogen concentration is saturated, and 4 pieces of saturated hydrogen concentration samples are obtained and placed in a liquid nitrogen tank for standby use;
[0119] (11) Loading head radius: The sample thickness is 1.0 mm and the radius R is set to 5 mm;
[0120] (12) Determination of reference stress: After thawing, the saturated hydrogen concentration sample was loaded using a U-bending test machine. The loading head was selected by calculation to load different stresses. The loading time was 5 min. The loading stress started from 0.2 times the tensile strength, i.e., 275 MPa. The stress was gradually increased until the saturated hydrogen concentration sample cracked. The stress at this time was the reference stress of 540 MPa.
[0121] (13) Preparation of hydrogen charging samples: Prepare hydrogen charging samples with hydrogen concentrations of 0.1 ppm, 0.2 ppm, 0.3 ppm, and 0.5 ppm using the hydrogen concentration curve, and place them in a liquid nitrogen tank for standby use;
[0122] (14) Test stress of hydrogen-filled samples: Based on the initial stress, the formula K 初 =(1.2-C H / C m )×K, the initial stresses of several groups of samples were 595MPa, 540MPa, 485MPa, and 380MPa respectively;
[0123] (15) Threshold hydrogen concentration measurement and hydrogen resistance performance determination: Using a U-bend test machine, samples with different hydrogen concentrations were selected for bending tests. The initial stress of the test was determined by the formula in step 14. The test stress head selection and steps were carried out with reference to steps 11 and 12. The four groups of hydrogen-charged samples did not break after loading the initial stress. The stress was then increased from 0.4 times the tensile strength until the hydrogen-charged samples cracked. The test results are shown in Table 3. It can be seen that under the condition of a hydrogen concentration of 0.1 ppm, the minimum breaking stress reached 1087 MPa, reaching 0.83 times the tensile strength. The ratio of the minimum breaking stress to the tensile strength exceeded 0.8. The hydrogen-charged samples with this hydrogen concentration met the requirements, while the other hydrogen-charged samples did not meet the requirements. Thus, the threshold hydrogen concentration of MS1300 cold-rolled sheet was 0.1 ppm.
[0124] Table 3
[0125]
[0126] The metal material in the present invention is mainly high-strength automobile steel as the research object, and it is also applicable to other high-strength metal materials. The method can be directly used for high-strength steel bare plates, and the method can only be used for high-strength steel or metal materials with coated surfaces after the surface coating is removed by a suitable method without changing the material structure.
[0127] Through the above process, the present invention can obtain the threshold hydrogen concentration of different metal materials and the minimum breaking stress of metal materials under different hydrogen concentration conditions, and can quantify the hydrogen embrittlement risk to a certain extent through the relationship between hydrogen concentration and stress, and more directly clarify the anti-purification ability of metal materials. The relationship curve between stress and hydrogen concentration obtained by the method of the present invention can be used to guide the use of metal materials (such as high-strength steel), and can also evaluate the hydrogen embrittlement risk of metal materials in actual use, so as to take timely measures to reduce the use risk of metal materials (such as high-strength steel).
[0128] In summary, the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solutions of the present invention, which should be included in the scope of the claims of the present invention.
Claims
1. A method for evaluating the hydrogen resistance of a metal material, characterized in that: The following steps are involved: S1, preparing a metal material into a sample, and removing free hydrogen in the sample by heating; S2, tensile strength measurement, determining the tensile strength of the sample by a slow tensile test; S3, removing hydrogen by thermal desorption, removing diffusible hydrogen in the sample by thermal desorption; S4, electrochemical hydrogen charging, using the electrochemical method to place the dehydrogenated sample in a hydrogen charging solution for different lengths of time; S5, measuring the saturated hydrogen concentration, measuring the hydrogen of the samples obtained in step S4 one by one according to the hydrogen charging time, determining the saturated hydrogen concentration of the samples by comparison, and establishing a hydrogen charging concentration change curve; S6, according to the hydrogen charging concentration change curve obtained in step S5, a plurality of hydrogen-charged samples with different hydrogen concentrations are prepared, and bending tests with different stresses are performed respectively to obtain the minimum compressive stress of the hydrogen-charged sample with each hydrogen concentration, and the hydrogen resistance of the metal material is judged accordingly.
2. The method for evaluating the hydrogen resistance of a metal material according to claim 1, characterized in that: In step S1: The sample is surface treated with acetone ultrasound for a treatment time of >15 min; and / or During the heating process, the heating temperature is 150-200° C. and the heating time is 15-120 min; and / or After the heat treatment, the free hydrogen concentration in the sample was reduced to below 0.02 ppm.
3. The method for evaluating the hydrogen resistance of a metal material according to claim 1, characterized in that: In the step S3, during the dehydrogenation process by thermal desorption, the sample is heated to 400° C. and maintained for 20 to 60 minutes.
4. The method for evaluating the hydrogen resistance of a metal material according to claim 1, characterized in that: In step S4: The hydrogen charging solution is 0.5 mol / L H2SO4+0.3 g / L thiourea solution; and / or The hydrogen charging current during the electrochemical hydrogen charging process is 10 mA / cm 2 and / or The hydrogen charging times of different lengths are 10 to 600 minutes.
5. The method for evaluating the hydrogen resistance of a metal material according to claim 1, characterized in that: In step S5, during the saturated hydrogen concentration determination process, the difference between the hydrogen contents of the samples with different hydrogen filling time is compared until the difference between the hydrogen contents of the samples with different hydrogen filling time is less than 0.1 ppm. The hydrogen content at this time is the saturated hydrogen concentration of the sample.
6. The method for evaluating the hydrogen resistance of a metal material according to claim 1, characterized in that: In step S6: The hydrogen concentration of the hydrogen-filled samples with different hydrogen concentrations is 0.02 to 0.8 times the saturated hydrogen concentration; and / or During the bending test, the hydrogen-filled sample is loaded with different stresses, the radius of the loading pressure head is 4 to 5 times the sample thickness, and the loading time is controlled within 20 minutes.
7. The method for evaluating the hydrogen resistance of a metal material according to claim 6, characterized in that: In the step S6, during the bending test, if the hydrogen-charged sample does not crack after the initial stress loading is performed on the hydrogen-charged sample, the stress is sequentially increased from 0.4 times the tensile strength until the hydrogen-charged sample cracks, and the stress at this time is the minimum compressive stress of the hydrogen-charged sample.
8. The method for evaluating the hydrogen resistance of a metal material according to claim 7, characterized in that: In step S6, the calculation formula of the initial stress of the bending test is as follows: K 初 =(1.2-C H / C m )×K; Among them, K 初 is the initial stress, in MPa; C H is the hydrogen concentration of the hydrogen-filled sample, in ppm; C m is the saturated hydrogen concentration of the sample, in ppm; K is the reference stress, in MPa.
9. The method for evaluating the hydrogen resistance of a metal material according to claim 8, characterized in that: In step S6, the reference stress is determined by the following steps: Electrochemically charging the sample after dehydrogenation treatment according to the hydrogen charging concentration variation curve to charge the sample to a saturated hydrogen concentration, thereby obtaining a saturated hydrogen concentration sample; The saturated hydrogen concentration sample is subjected to a bending test, and different stresses are loaded on the saturated hydrogen concentration sample. The stress loading time is controlled within 20 minutes, and the loading stress is increased from 0.2 times the tensile strength to 0.3 to 1.0 times the tensile strength in sequence until the saturated hydrogen concentration sample breaks. The stress when the saturated hydrogen concentration sample breaks is recorded as the reference stress K.
10. The method for evaluating the hydrogen resistance of a metal material according to any one of claims 1 to 9, characterized in that: In step S6, the hydrogen resistance of the metal material is determined by the following method: The ratio of the minimum compressive stress to the tensile strength of the hydrogen-charged sample is calculated. When the ratio is ≥0.8, the hydrogen-charged sample has qualified hydrogen resistance. At this time, the hydrogen concentration corresponding to the hydrogen-charged sample with qualified hydrogen resistance is the threshold hydrogen concentration of the metal material.