Preparation method and application of conductive paste for carbon-coated aluminum foil

By introducing acrylic groups and sulfonic acid groups into lithium-ion batteries, combined with electrospinning technology, the problem of insufficient adhesion between conductive paste and positive electrode active material is solved, and the use of lithium batteries is improved Lifespan and energy density.

CN119008080APending Publication Date: 2024-11-22GUANGDONG LEARY NEW MATERIAL TECHNOLOGY CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411115901.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In existing lithium-ion batteries, the adhesion between the conductive paste and the positive electrode active material is insufficient, resulting in easy separation during charging and discharging, increasing the internal resistance of the lithium battery and affecting the service life and safety performance.

Method used

A conductive paste preparation method is adopted to introduce acrylic groups and sulfonic acid groups by polymerizing in an inert atmosphere to improve the uniformity of charge distribution, and to uniformly spray the conductive paste with an electrospinning device to enhance the bonding force and peel strength.

Benefits of technology

The bonding force and peel strength between the conductive paste and the positive electrode active material are significantly improved, the service life of the lithium battery is extended and the energy density of the battery is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004993607400000121
    Figure BDA0004993607400000121
  • Figure BDA0004993607400000122
    Figure BDA0004993607400000122
Patent Text Reader

Abstract

The invention relates to the technical field of conductive paste, and discloses a preparation method and application of conductive paste for a carbon-coated aluminum foil. S1) preparing a reaction solution; s2) preparing a binder; s3) adding the binder into a mixed solution of a conductive agent, an auxiliary agent, a solvent and deionized water to prepare the conductive slurry; the first monomer comprises one or two of acrylic acid, methacrylic acid, methyl acrylate, ethyl acrylate, methyl methacrylate and ethyl methacrylate; the second monomer comprises one or two of potassium 2, 5-dihydroxybenzenesulfonate, sodium sulfonate, sodium methanesulfonate, chlorosulfonic acid, sodium 2-thioethanesulfonate, sulfonamide, potassium methanesulfonate, potassium sulfamate and potassium trifluoromethanesulfonate. The sulfonic acid group and the acrylic acid group generate a conjugation effect, so that the uniformity of charge distribution of the conductive slurry can be improved, and the binding power of a conductive slurry coating and a positive electrode active material coating is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of conductive pastes, and in particular to a preparation method of conductive paste for carbon-coated aluminum foil and application thereof. Background Art

[0002] Lithium-ion batteries have the advantages of small size and high energy density and are widely used in new energy vehicles.

[0003] The prior art lithium-ion battery uses a carbon-coated aluminum foil coated with a conductive slurry on the surface instead of the early rolled aluminum foil as the positive electrode current collector to suppress the polarization of the lithium-ion battery, thereby achieving the purpose of reducing the thermal effect and improving the rate performance of the lithium-ion battery.

[0004] In the carbon-coated aluminum foil of the prior art, the bonding force between the conductive paste used and the coated positive electrode active material is insufficient. After multiple charges and discharges, the conductive paste and the positive electrode active material are easily separated due to thermal expansion, resulting in an increase in the internal resistance of the lithium battery, affecting the service life and safety performance of the lithium battery. Summary of the invention

[0005] In view of the above problems, the first object of the present invention is to provide a method for preparing a conductive paste to solve the problem of insufficient bonding between the conductive paste and the coated positive electrode active material.

[0006] The second object of the present invention is to provide a method for preparing a conductive slurry using the above preparation method to improve the peel strength between the carbon-coated aluminum foil and the positive electrode active material coating.

[0007] To achieve this object, the present invention adopts the following technical solutions:

[0008] A method for preparing a conductive paste comprises the following steps:

[0009] S1) adding deionized water to a reaction kettle in an inert atmosphere, stirring and heating to a reaction temperature, and sequentially adding a first monomer and an initiator dropwise, and completing the reaction to obtain a reaction solution;

[0010] S2) adding deionized water, a mixed solution of a second monomer and an initiator dropwise to the reaction solution, and after the reaction is completed, cooling the solution to room temperature and discharging the solution to obtain a binder;

[0011] S3) adding the binder to a mixed solution of a conductive agent, an auxiliary agent, a solvent and deionized water, and dispersing the mixture evenly to obtain the conductive paste;

[0012] The first monomer includes one or two of acrylic acid, methacrylic acid, methyl acrylate, ethyl acrylate, methyl methacrylate and ethyl methacrylate;

[0013] The second monomer includes one or two of potassium 2,5-dihydroxybenzenesulfonate, sodium sulfonate, sodium methanesulfonate, chlorosulfonic acid, sodium 2-mercaptoethanesulfonate, sulfonamide, potassium methanesulfonate, potassium sulfamate and potassium trifluoromethanesulfonate.

[0014] Specifically, in step S1), 50-80 parts of deionized water, 5-15 parts of the first monomer, and 0.001-0.005 parts of the initiator are added; the reaction temperature is 50-80° C., the dropwise addition time is 1.5-3 hr, and the reaction time is 1.5-1 hr.

[0015] Furthermore, in step S2), the mixed solution contains 15-20 parts of deionized water, 1-5 parts of the second monomer and 0.01-0.1 parts of the initiator; the reaction temperature is 50-80° C., the dropping time is 1.5-3 hr, and the reaction time is 2.5-4 hr.

[0016] Preferably, the initiator is one or two of sodium persulfate, potassium persulfate, hydrogen peroxide and ammonium persulfate.

[0017] Specifically, calculated by weight, the conductive paste includes 40-60 parts of deionized water, 5-15 parts of solvent, 30-50 parts of binder, 2-5 parts of conductive agent and 0.1-0.5 parts of auxiliary agent.

[0018] Preferably, the solvent is one or two of isopropanol, n-butanol, isobutanol and n-hexanol;

[0019] The auxiliary agent is one or two of polyvinyl pyrrolidone, cetyltrimethylammonium bromide, cetyltrimethylammonium chloride, polyoxyethylene sorbitol ester and polyethylene glycol.

[0020] Preferably, the conductive agent is one or two of carbon black, graphite, superconducting carbon black, Ketjen black, graphene and carbon nanotubes.

[0021] Preferably, in step S1), the inert atmosphere is a nitrogen atmosphere and / or an argon atmosphere.

[0022] Furthermore, the present invention provides a method for using a conductive paste, using the conductive paste prepared by the above-mentioned method for preparing the conductive paste to prepare a positive electrode current collector, the steps are as follows:

[0023] The conductive slurry is injected into an injection needle tube, the conductive slurry is evenly sprayed on the aluminum foil through an electrostatic spinning device, and dried to obtain a carbon-coated aluminum foil coated with the conductive slurry;

[0024] The positive electrode active material is uniformly coated on the surface of the carbon-coated aluminum foil, and then rolled and dried to obtain the positive electrode current collector;

[0025] Calculated by weight, the positive electrode active material includes 45-55 parts of lithium iron phosphate, 4-6 parts of conductive carbon black, 2-3 parts of polyvinylidene fluoride and 40-45 parts of N-methylpyrrolidone.

[0026] The beneficial effect of the technical solution of the method for preparing a conductive paste of the present invention is that the method for preparing the conductive paste improves the uniformity of charge distribution when using the conductive paste by introducing acrylic acid groups and sulfonic acid groups with conjugated effects, so as to improve the adhesion and peeling strength between the conductive paste coating and the positive electrode active material coating.

[0027] Furthermore, the method for using the conductive slurry proposed in the present invention is to evenly spray the conductive slurry on aluminum foil through an electrospinning device to improve the thickness uniformity, specific surface area and porosity of the obtained carbon-coated aluminum foil, thereby improving the peel strength between the carbon-coated aluminum foil and the positive electrode active material coating, as well as the energy density of the battery. DETAILED DESCRIPTION

[0028] The technical solution of the present invention is further illustrated below through specific implementation methods.

[0029] In the description of this specification, the description with reference to the terms "embodiment", "example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0030] Although the embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the claims and their equivalents.

[0031] A method for preparing a conductive paste comprises the following steps:

[0032] S1) adding deionized water to a reaction kettle in an inert atmosphere, stirring and heating to a reaction temperature, and sequentially adding a first monomer and an initiator dropwise, and completing the reaction to obtain a reaction solution;

[0033] S2) adding deionized water, a mixed solution of a second monomer and an initiator dropwise to the reaction solution, and after the reaction is completed, cooling the solution to room temperature and discharging the solution to obtain a binder;

[0034] S3) adding the binder to a mixed solution of a conductive agent, an auxiliary agent, a solvent and deionized water, and dispersing the mixture evenly to obtain the conductive paste;

[0035] The first monomer includes one or two of acrylic acid, methacrylic acid, methyl acrylate, ethyl acrylate, methyl methacrylate and ethyl methacrylate;

[0036] The second monomer includes one or two of potassium 2,5-dihydroxybenzenesulfonate, sodium sulfonate, sodium methanesulfonate, chlorosulfonic acid, sodium 2-mercaptoethanesulfonate, sulfonamide, potassium methanesulfonate, potassium sulfamate and potassium trifluoromethanesulfonate.

[0037] The preparation method of the conductive paste of the present invention introduces an acrylic acid group into the first monomer and a sulfonic acid group into the second monomer. The sulfonic acid group has electron-withdrawing properties and produces a conjugated effect with the acrylic acid group, which can improve the uniformity of charge distribution when using the conductive paste, thereby improving the adhesion between the conductive paste coating and the positive electrode active material coating, and further improving the peel strength between the carbon-coated aluminum foil and the positive electrode active material coating.

[0038] Specifically, in step S1), 50-80 parts of deionized water, 5-15 parts of the first monomer, and 0.001-0.005 parts of the initiator are added; the reaction temperature is 50-80° C., the dropwise addition time is 1.5-3 hr, and the reaction time is 1.5-1 hr.

[0039] Specifically, in step S2), the mixed solution contains 15-20 parts of deionized water, 1-5 parts of the second monomer and 0.01-0.1 parts of the initiator; the reaction temperature is 50-80° C., the dropwise addition time is 1.5-3 hr, and the reaction time is 2.5-4 hr.

[0040] Preferably, the initiator is one or two of sodium persulfate, potassium persulfate, hydrogen peroxide and ammonium persulfate.

[0041] With deionized water as the medium, the first monomer or the second monomer is polymerized under the action of an initiator, and the reaction speed is controlled by dripping to reduce the monomer residual rate in the polymer and improve the distribution uniformity and stability of the conductive paste in the carbon-coated aluminum foil.

[0042] Specifically, calculated by weight, the conductive paste includes 40-60 parts of deionized water, 5-15 parts of solvent, 30-50 parts of binder, 2-5 parts of conductive agent and 0.1-0.5 parts of auxiliary agent.

[0043] Preferably, the solvent is one or two of isopropanol, n-butanol, isobutanol and n-hexanol;

[0044] The auxiliary agent is one or two of polyvinyl pyrrolidone, cetyltrimethylammonium bromide, cetyltrimethylammonium chloride, polyoxyethylene sorbitol ester and polyethylene glycol.

[0045] The added solvent and additive are used to improve the dissolution and dispersion uniformity of the binder and the conductive agent in the deionized water, thereby improving the distribution uniformity and adhesion effect of the conductive paste on the surface of the aluminum foil.

[0046] Preferably, the conductive agent is one or two of carbon black, graphite, superconducting carbon black, Ketjen black, graphene and carbon nanotubes.

[0047] The above conductive agents have a large specific surface area, which helps to improve the conductivity of the carbon-coated aluminum foil and helps to improve the bonding force between the carbon-coated aluminum foil and the positive electrode active material, thereby increasing the service life of the positive electrode current collector.

[0048] Preferably, in step S1), the inert atmosphere is a nitrogen atmosphere and / or an argon atmosphere.

[0049] The polymerization reaction of the first monomer and the second monomer is carried out under an inert atmosphere of nitrogen and / or argon to avoid the influence of oxygen in the air on the properties of the polymer.

[0050] Furthermore, the present invention provides a method for using a conductive paste, using the conductive paste prepared by the above-mentioned method for preparing the conductive paste to prepare a positive electrode current collector, the steps are as follows:

[0051] The conductive slurry is injected into an injection needle tube, the conductive slurry is evenly sprayed on the aluminum foil through an electrostatic spinning device, and dried to obtain a carbon-coated aluminum foil coated with the conductive slurry;

[0052] The positive electrode active material is uniformly coated on the surface of the carbon-coated aluminum foil, and then rolled and dried to obtain the positive electrode current collector;

[0053] Calculated by weight, the positive electrode active material includes 45-55 parts of lithium iron phosphate, 4-6 parts of conductive carbon black, 2-3 parts of polyvinylidene fluoride and 40-45 parts of N-methylpyrrolidone.

[0054] The resistance of the prepared carbon-coated aluminum foil is 0.004±0.0005Ω. The vertical peeling method is used on a tensile testing machine to measure the peeling strength between the conductive slurry coating of the positive electrode current collector and the positive electrode active material coating to be 1450±200N / m, indicating strong adhesion.

[0055] Examples 1-5 and Comparative Example 1

[0056] Example 1

[0057] 1.1 The conductive paste for carbon-coated aluminum foil of Example 1 was prepared according to the following steps:

[0058] S1) adding 55 parts of deionized water to a reactor in a nitrogen atmosphere, stirring at a rate of 50 r / min, and heating the deionized water to 50-80° C., and sequentially dropping 5 parts of acrylic acid monomer and 0.001 parts of sodium persulfate, the dropping time is 1.5 hours, and reacting for 0.5 hours to obtain a reaction solution of Example 1;

[0059] S2) adding dropwise a mixed solution of 1 part sodium sulfonate, 0.01 part potassium persulfate and 15 parts deionized water to the reaction solution of Example 1 for 1 hour. After reacting for 2.5 hours, cooling to room temperature and discharging the material to obtain the binder of Example 1;

[0060] S3) 8 parts of Ketjen black, 1 part of graphene, 0.05 parts of polyvinyl pyrrolidone and 25 parts of deionized water were stirred and mixed, and dispersed at high speed for 40 minutes to obtain a first solution;

[0061] S4) 35 parts of the binder of Example 1 are mixed with 40 parts of deionized water, and dispersed at high speed for 20 minutes to obtain a second solution, and then the first solution is added to the second solution, and dispersed at high speed again for 30 minutes to obtain the conductive paste of Example 1.

[0062] 1.2 The conductive slurry of Example 1 was injected into a syringe with a needle inner diameter of 0.15 mm in an electrospinning device, and aluminum foil was covered on the collector. The positive voltage of the electrospinning device was 15 KV, and the negative voltage was -4 KV. The injection speed was 0.5 m / min, and the distance between the stainless steel needle tip and the collector was 16 cm. The collector speed was 13 r / min. The above-mentioned conductive slurry was evenly sprayed on the aluminum foil. After collecting for 5 hours, it was dried in an oven at 85°C for 1 hour to obtain the carbon-coated aluminum foil of Example 1.

[0063] 1.2.1 The surface resistance of the carbon-coated aluminum foil of Example 1 was tested using a pole piece resistance meter. The test results are shown in Table 1.

[0064] 1.3 The positive electrode active material is uniformly coated on the surface of the carbon-coated aluminum foil of Example 1, rolled and dried to obtain the positive electrode current collector of Example 1.

[0065] 1.3.1 The above positive electrode active material composition is: 50 parts of lithium iron phosphate, 5 parts of conductive carbon black, 2 parts of polyvinylidene fluoride and 43 parts of N-methylpyrrolidone.

[0066] 1.3.2 The vertical peeling method was used on a tensile testing machine to test the peeling strength between the conductive slurry coating and the positive electrode active material coating of Example 1. The test results are shown in Table 3.

[0067] Example 2

[0068] 2.1 Prepare the conductive paste of Example 2 according to the following steps:

[0069] T1) mixing 8 parts of carbon nanotubes, 1 part of graphene, 0.05 parts of polyvinyl pyrrolidone and 25 parts of deionized water, and dispersing at high speed for 40 minutes to obtain a third solution;

[0070] T2) 35 parts of the binder of Example 1 were mixed with 40 parts of deionized water, and dispersed at high speed for 20 minutes to obtain a fourth solution, and then the third solution was mixed with the fourth solution and dispersed at high speed for 30 minutes to obtain the conductive paste of Example 2.

[0071] 2.2 The conductive slurry of Example 2 was injected into a syringe with a needle inner diameter of 0.15 mm in an electrospinning device, and aluminum foil was covered on the collector. The positive voltage of the electrospinning device was 15 KV, and the negative voltage was -4 KV. The injection speed was 0.5 m / min, and the distance between the stainless steel needle tip and the collector was 16 cm. The collector speed was 13 r / min. The above-mentioned conductive slurry was evenly sprayed on the aluminum foil. After collecting for 5 hours, it was dried in an oven at 85°C for 1 hour to obtain the carbon-coated aluminum foil of Example 2.

[0072] 2.3 The positive electrode active material is uniformly coated on the surface of the carbon-coated aluminum foil of Example 2, rolled and dried to obtain the positive electrode current collector of Example 2.

[0073] 2.3.1 The above positive electrode active material composition is: 50 parts of lithium iron phosphate, 5 parts of conductive carbon black, 2 parts of polyvinylidene fluoride and 43 parts of N-methylpyrrolidone.

[0074] 2.3.2 The vertical peeling method was used on a tensile testing machine to test the peeling strength between the conductive slurry coating and the positive electrode active material coating of Example 2. The test results are shown in Table 3.

[0075] Example 3

[0076] 3.1 Prepare the conductive paste of Example 3 according to the following steps:

[0077] U1) 8 parts of carbon black, 1 part of graphite, 0.05 parts of polyvinyl pyrrolidone and 25 parts of deionized water were mixed and dispersed at high speed for 40 minutes to obtain a fifth solution;

[0078] U2) 35 parts of the binder of Example 1 were mixed with 40 parts of deionized water, and dispersed at high speed for 20 minutes to obtain a sixth solution. The fifth solution and the sixth solution were mixed, and dispersed at high speed for another 30 minutes to obtain the conductive paste of Example 3.

[0079] 3.2 The conductive slurry of Example 3 was injected into a syringe with an inner diameter of 0.15 mm in the needle of an electrospinning device, and the collector was covered with aluminum foil. The positive voltage of the electrospinning device was 15 KV, and the negative voltage was -4 KV. The injection speed was 0.5 m / min, and the distance between the stainless steel needle tip and the collector was 16 cm. The collector speed was 13 r / min. The above-mentioned conductive slurry was evenly sprayed on the aluminum foil. After collecting for 5 hours, it was dried in an oven at 85°C for 1 hour to obtain the carbon-coated aluminum foil of Example 3.

[0080] 3.3 The positive electrode active material is uniformly coated on the surface of the carbon-coated aluminum foil of Example 3, rolled and dried to obtain the positive electrode current collector of Example 3.

[0081] 3.3.1 The above positive electrode active material composition is: 50 parts of lithium iron phosphate, 5 parts of conductive carbon black, 2 parts of polyvinylidene fluoride and 43 parts of N-methylpyrrolidone.

[0082] 3.3.2 The vertical peeling method was used on a tensile testing machine to test the peeling strength between the conductive slurry coating and the positive electrode active material coating of Example 3. The test results are shown in Table 3.

[0083] Example 4

[0084] 4.1 The conductive paste of Example 4 was prepared according to the following steps:

[0085] V1) adding 55 parts of deionized water to a reactor in a nitrogen atmosphere, stirring at a rate of 50 r / min, and heating the deionized water to 50-80° C., and sequentially dropping 5 parts of acrylic acid monomer and 0.001 parts of sodium persulfate, the dropping time is 1.5 hours, and the reaction is carried out for 0.5 hours to obtain a reaction solution of Example 4;

[0086] V2) In the reaction solution of Example 4, a mixture of 1 part of chlorosulfonic acid, 0.01 part of ammonium persulfate and 15 parts of deionized water was added dropwise for 1 hour. After reacting for 2.5 hours, the mixture was cooled to room temperature and discharged to obtain the binder of Example 4;

[0087] V3) 6 parts of superconducting carbon black, 3 parts of graphite, 0.1 parts of polyethylene glycol and 30 parts of deionized water were stirred and mixed, and dispersed at high speed for 40 minutes to obtain a seventh solution;

[0088] V4) 35 parts of the binder of Example 4 were mixed with 40 parts of deionized water, and dispersed at high speed for 20 minutes to obtain an eighth solution. The seventh solution was then added to the eighth solution, and dispersed at high speed again for 30 minutes to obtain the conductive paste of Example 4.

[0089] 4.2 The conductive slurry of Example 4 was injected into a syringe with a needle inner diameter of 0.15 mm in an electrospinning device, and aluminum foil was covered on the collector. The positive voltage of the electrospinning device was 15 KV, and the negative voltage was -4 KV. The injection speed was 0.5 m / min, and the distance between the stainless steel needle tip and the collector was 16 cm. The collector speed was 13 r / min. The above-mentioned conductive slurry was evenly sprayed on the aluminum foil. After collecting for 5 hours, it was dried in an oven at 85°C for 1 hour to obtain the carbon-coated aluminum foil of Example 4.

[0090] 4.3 The positive electrode active material is uniformly coated on the surface of the carbon-coated aluminum foil of Example 4, rolled and dried to obtain the positive electrode current collector of Example 4.

[0091] 4.3.1 The above positive electrode active material composition is: 50 parts of lithium iron phosphate, 5 parts of conductive carbon black, 2 parts of polyvinylidene fluoride and 43 parts of N-methylpyrrolidone.

[0092] 4.3.2 The vertical peeling method was used on a tensile testing machine to test the peeling strength between the conductive slurry coating and the positive electrode active material coating of Example 4. The test results are shown in Table 3.

[0093] Example 5

[0094] 5.1 Prepare the conductive paste of Example 5 according to the following steps:

[0095] W1) 8 parts of superconducting carbon black, 1 part of graphite, 0.05 parts of polyethylene glycol and 25 parts of deionized water were mixed and dispersed at high speed for 40 minutes to obtain a ninth solution;

[0096] W2) 35 parts of the binder of Example 4 were mixed with 40 parts of deionized water, and dispersed at high speed for 20 minutes to obtain a tenth solution. The ninth solution was mixed with the tenth solution, and then dispersed at high speed for 30 minutes to obtain a conductive paste of Example 5.

[0097] 5.2 The conductive slurry of Example 5 was injected into a syringe with an inner diameter of 0.15 mm in the needle of an electrospinning device, and aluminum foil was covered on the collector. The positive voltage of the electrospinning device was 15 KV, and the negative voltage was -4 KV. The injection speed was 0.5 m / min, and the distance between the stainless steel needle tip and the collector was 16 cm. The collector speed was 13 r / min. The above-mentioned conductive slurry was evenly sprayed on the aluminum foil. After collecting for 5 hours, it was dried in an oven at 85°C for 1 hour to obtain the carbon-coated aluminum foil of Example 5.

[0098] 5.3 The positive electrode active material is uniformly coated on the surface of the carbon-coated aluminum foil of Example 5, rolled and dried to obtain the positive electrode current collector of Example 5.

[0099] 5.3.1 The above positive electrode active material composition is: 50 parts of lithium iron phosphate, 5 parts of conductive carbon black, 2 parts of polyvinylidene fluoride and 43 parts of N-methylpyrrolidone.

[0100] 5.3.2 The vertical peeling method was used on a tensile testing machine to test the peeling strength between the conductive slurry coating and the positive electrode active material coating of Example 5. The test results are shown in Table 3.

[0101] Comparative Example 1

[0102] 6.1 Prepare the conductive paste of Comparative Example 1 according to the following steps:

[0103] 30 parts of polyacrylic acid resin emulsion, 0.2 parts of sodium carboxymethyl cellulose, 1 part of graphite, 3 parts of carbon black and 66 parts of deionized water were stirred and mixed, and dispersed at high speed for 40 minutes to prepare the conductive paste of Comparative Example 1.

[0104] 6.2 The conductive paste of Comparative Example 1 was sprayed uniformly on the aluminum foil, and then dried in an oven at 85° C. for 1 h to obtain the carbon-coated aluminum foil of Comparative Example 1.

[0105] 6.2.1 The surface resistance of the carbon-coated aluminum foil of Comparative Example 1 was tested using a pole piece resistance meter. The test results are shown in Table 2.

[0106] 6.3 The positive electrode active material is uniformly coated on the surface of the carbon-coated aluminum foil of Comparative Example 1, rolled and dried to obtain the positive electrode current collector of Comparative Example 1.

[0107] 6.3.1 The above positive electrode active material composition is: 50 parts of lithium iron phosphate, 5 parts of conductive carbon black, 2 parts of polyvinylidene fluoride and 43 parts of N-methylpyrrolidone.

[0108] 6.3.2 The vertical peeling method was used on a tensile testing machine to test the peeling strength between the conductive slurry coating and the positive electrode active material coating of Comparative Example 1. The test results are shown in Table 3.

[0109] Table 1 Resistance test results of Example 1

[0110]

[0111] Table 2 Resistance test results of comparative example 1

[0112]

[0113] Table 3 Peel strength test results of Examples 1-5 and Comparative Example 1

[0114] Example or comparative example number Peel strength (N / m) Example 1 1500 Example 2 1640 Example 3 1190 Example 4 1260 Example 5 1380 Comparative Example 1 140

[0115] In summary, the preparation method of the conductive paste improves the uniformity of charge distribution using the conductive paste by introducing acrylic acid groups and sulfonic acid groups with conjugated effects, so as to improve the bonding force and peeling strength between the conductive paste coating and the positive electrode active material coating.

[0116] Furthermore, the present invention proposes a method for using the above-mentioned conductive slurry, in which the conductive slurry is evenly sprayed on aluminum foil through an electrospinning device to improve the thickness uniformity, specific surface area and porosity of the obtained carbon-coated aluminum foil, thereby improving the peel strength between the carbon-coated aluminum foil and the positive electrode active material coating, as well as the energy density of the battery.

[0117] The technical principle of the present invention is described above in conjunction with specific embodiments. These descriptions are only for explaining the principle of the present invention and cannot be interpreted as limiting the scope of protection of the present invention in any way. Based on the explanations herein, those skilled in the art can associate other specific implementations of the present invention without paying creative labor, and these methods will fall within the scope of protection of the present invention.

Claims

1. A method for preparing a conductive paste, characterized in that: The following steps are included: S1) adding deionized water to a reactor in an inert atmosphere, stirring and heating to a reaction temperature, and sequentially adding a first monomer and an initiator dropwise until the reaction is complete to obtain a reaction solution; S2) adding a mixed solution of deionized water, a second monomer, and an initiator dropwise to the reaction solution, and after the reaction is completed, cooling the solution to room temperature and discharging the solution to obtain a binder; S3) adding the binder to a mixed solution of a conductive agent, an additive, a solvent and deionized water, and dispersing the mixture evenly to obtain the conductive paste; The first monomer comprises one or two of acrylic acid, methacrylic acid, methyl acrylate, ethyl acrylate, methyl methacrylate and ethyl methacrylate; The second monomer includes one or two of potassium 2,5-dihydroxybenzenesulfonate, sodium sulfonate, sodium methanesulfonate, chlorosulfonic acid, sodium 2-mercaptoethanesulfonate, sulfonamide, potassium methanesulfonate, potassium sulfamate and potassium trifluoromethanesulfonate.

2. The method for preparing the conductive paste according to claim 1, wherein: In step S1), 50-80 parts of deionized water, 5-15 parts of the first monomer, and 0.001-0.005 parts of the initiator are added; the reaction temperature is 50-80° C., the dropwise addition time is 1.5-3 hours, and the reaction time is 1.5-1 hour.

3. The method for preparing the conductive paste according to claim 1, wherein: In step S2), the mixed solution contains 15-20 parts of deionized water, 1-5 parts of the second monomer, and 0.01-0.1 parts of the initiator; the reaction temperature is 50-80° C., the dropwise addition time is 1.5-3 hours, and the reaction time is 2.5-4 hours.

4. The method for preparing the conductive paste according to claim 1, wherein: The initiator is one or two of sodium persulfate, potassium persulfate, hydrogen peroxide and ammonium persulfate.

5. The method for preparing the conductive paste according to claim 1, wherein: Calculated by weight, the conductive paste includes 40-60 parts of deionized water, 5-15 parts of solvent, 30-50 parts of binder, 2-5 parts of conductive agent and 0.1-0.5 parts of auxiliary agent.

6. The method for preparing the conductive paste according to claim 1, wherein: The solvent is one or two of isopropyl alcohol, n-butanol, isobutanol and n-hexanol; The auxiliary agent is one or two of polyvinyl pyrrolidone, cetyltrimethylammonium bromide, cetyltrimethylammonium chloride, polyoxyethylene sorbitol ester and polyethylene glycol.

7. The method for preparing the conductive paste according to claim 1, wherein: The conductive agent is one or two of carbon black, graphite, superconducting carbon black, Ketjen black, graphene and carbon nanotubes.

8. The method for preparing the conductive paste according to claim 1, wherein: In step S1), the inert atmosphere is a nitrogen atmosphere and / or an argon atmosphere.

9. A method for using a conductive paste, characterized in that: The conductive paste prepared by the method for preparing the conductive paste according to any one of claims 1 to 8 is used to prepare a positive electrode current collector, and the steps are as follows: The conductive slurry is injected into an injection needle tube, the conductive slurry is evenly sprayed on the aluminum foil by an electrospinning device, and then dried to obtain a carbon-coated aluminum foil coated with the conductive slurry; The positive electrode active material is uniformly coated on the surface of the carbon-coated aluminum foil, and then rolled and dried to obtain the positive electrode current collector; Calculated by weight, the positive electrode active material includes 45-55 parts of lithium iron phosphate, 4-6 parts of conductive carbon black, 2-3 parts of polyvinylidene fluoride and 40-45 parts of N-methylpyrrolidone.