Chip tantalum capacitor and preparation method thereof
By forming a MnO2 layer on the surface of the tantalum core of the tantalum capacitor and using surface treatment agents such as silane coupling agents, the interface bonding force between the graphite layer and the silver paste layer is improved, and the problem of insufficient bonding force in the prior art is solved, and high Performance and low cost tantalum capacitor preparation.
Patent Information
- Application Number
- CN202411175814.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-22
AI Technical Summary
The prior art is difficult to improve the interface bonding force of tantalum capacitors without changing the material formulation of the graphite layer and the silver paste layer or improving the preparation process, and there is a high manufacturing cost and impact on other properties.
After hydrolysis treatment, the silver paste layer is impregnated to improve the interface bond between the graphite layer and the silver paste layer by forming an MnO2 layer on the surface of the tantalum core and using a mixture of silane coupling agent, anhydrous ethanol and deionized water as the surface treatment agent. force.
It significantly improves the interface bonding force between the graphite layer and the silver paste layer, extends the service life of tantalum capacitors, reduces manufacturing costs, and meets the needs of high performance and low cost.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of capacitor manufacturing, and in particular relates to a chip-type tantalum capacitor and a preparation method thereof. Background Art
[0002] Tantalum capacitors are an important electronic component, widely used in various electronic devices. Its main structure includes an anode, a dielectric film and a cathode. Among them, the graphite layer is mainly used as a conductive layer. It is located on the cathode material of the capacitor (such as a conductive polymer or manganese dioxide). The silver paste layer is impregnated on the graphite layer and connected to the lead frame to lead out the negative electrode. The interface bonding force between the graphite layer and the silver paste layer has an important influence on the performance of the tantalum capacitor. If the interface bonding force is insufficient, the tantalum capacitor may have problems such as unstable performance and shortened life during use. Therefore, how to improve the interface bonding force between the graphite layer and the silver paste layer is an important research direction in the field of tantalum capacitor manufacturing technology.
[0003] The existing solutions mainly change the material formula of the graphite layer and the silver paste layer or improve the preparation process to improve the interface bonding between the two. For example, the bonding state between the graphite layer and the silver paste layer can be improved by adding a specific binder or changing the sintering conditions. However, these methods often require complex operating processes and high costs, and may affect other properties of tantalum capacitors.
[0004] Although some solutions have been proposed in the prior art, there are still some problems and disadvantages. First, the existing solutions often require special equipment or materials, which increases the manufacturing cost of tantalum capacitors. Second, the existing solutions may affect other properties of tantalum capacitors, for example, the equivalent series resistance of tantalum capacitors may be increased. In addition, the existing solutions have limited effect on improving the interfacial bonding strength between the graphite layer and the silver paste layer, and sometimes even fail to meet the actual application requirements.
[0005] The patent document with announcement number CN116013576A discloses a conductive silver paste and a preparation method thereof, and in particular, relates to a polymer chip tantalum capacitor silver paste and a preparation method thereof. The method comprises: dissolving a mixture of several resins in a first solvent, stirring until completely dissolved, then adding an anti-settling agent and a curing agent, and obtaining an organic intermediate through centrifugal defoaming; sequentially adding flaky silver powder, carbon-based filler, silver-coated copper powder and the organic intermediate, filtering after three-roll grinding, and obtaining a slurry intermediate; adding a second solvent, a silane coupling agent and a defoaming agent to the slurry intermediate, and obtaining the slurry intermediate after centrifugal dispersion and defoaming. The method achieves the purpose of achieving a good combination of low equivalent series resistance and graphite layer on the basis of reducing costs by combining flaky silver powder, carbon-based filler and silver-coated copper powder and adopting a distributed preparation method. The patent requires a change in the material formula, which has a high transformation cost for enterprises with fixed production lines. At the same time, the specific ingredients used in the silane coupling agent and the corresponding use method are not disclosed.
[0006] The patent document with announcement number CN117995561A discloses a preparation method of an organic chip solid tantalum electrolytic capacitor, comprising the following steps: taking tantalum powder to press a tantalum block, and sintering it under vacuum conditions; impregnating the sintered block with an energy forming liquid, boiling and washing in a high-temperature steam environment, and then vacuum annealing, and then impregnating the original energy forming liquid and applying a DC voltage to obtain a tantalum core; impregnating the tantalum core with a silane coupling agent aqueous solution and then drying, repeatedly immersing it in a conductive polymer slurry and then drying, and then coating a graphite layer and a silver paste layer, and encapsulating it to obtain an organic chip solid tantalum electrolytic capacitor. The present invention improves the cycle stability of the capacitor through the conductive polymer slurry. In addition, by adopting a low-temperature formation method, it is subsequently placed in a high-temperature steam environment for boiling and washing and placed in a nitrogen environment for annealing, and the surface of the tantalum pentoxide dielectric layer is impregnated with a silane coupling agent aqueous solution, so as to effectively improve the stability of the tantalum pentoxide dielectric and improve the capacitor's ability to withstand high temperatures for a long time. Although the patent discloses that the silane coupling agent is γ-aminopropyltriethoxysilane, it does not disclose other types of silane coupling agents and the corresponding mass concentration ranges of the present application; and the technical problem to be solved by the patent is to improve the high temperature resistance of the capacitor, which is different from the present application. Summary of the invention
[0007] In order to solve the above technical problems, the present invention provides a chip-type tantalum capacitor and a preparation method thereof.
[0008] The present invention is achieved through the following technical solutions.
[0009] The present invention provides a method for preparing a chip tantalum capacitor, comprising the following steps:
[0010] Step 1: Pressing tantalum metal powder into tantalum blocks, and sintering the tantalum blocks in a vacuum environment;
[0011] Step 2: Form an oxide film on the surface of the sintered tantalum block, and then deposit MnO on the surface of the oxide film. 2 , we get MnO 2 layer;
[0012] Step 3: MnO 2 The surface of the layer is covered with a graphite layer to obtain a tantalum core, and then the tantalum core is immersed in a surface treatment agent;
[0013] Step 4: Drying and baking the tantalum core after being impregnated with the surface treatment agent;
[0014] Step 5: impregnate a layer of silver paste on the treated graphite layer of the tantalum core to form a silver paste layer;
[0015] Step 6: Perform curing treatment and test and evaluate the capacitor after preparation.
[0016] Preferably, in step S3, the surface treatment agent comprises a mixture of silane coupling agent, anhydrous ethanol and deionized water, the volume ratio of anhydrous ethanol to deionized water is 4-7:4-1, and the surface treatment agent is hydrolyzed for 0.5h-1h;
[0017] The silane coupling agent includes one or more of γ-aminopropyl-triethoxysilane, γ-glycidyloxypropyl-trimethoxysilane, γ-methacryloxy-trimethoxysilane, and vinyltrichlorosilane.
[0018] Preferably, the mass concentration of the one or more silane coupling agents is 15% to 25%.
[0019] Preferably, in step S1, the tantalum block is 2×10 -3 Pa~4×10 -3 Pa in a vacuum environment; in step S2, an anodic oxidation method is used to form Ta on the surface of the sintered tantalum block. 2 O 5 The dielectric oxide film is then thermally decomposed on Ta 2 O 5 MnO deposition on the surface of dielectric oxide film 2 .
[0020] Preferably, the immersion time in step S3 is 1 to 10 minutes.
[0021] Preferably, in step S4, the tantalum core impregnated with the surface treatment agent is dried at room temperature for 10 to 30 minutes, and then baked at 150° C. to 200° C. for 30 to 60 minutes.
[0022] Preferably, in step S5, the thickness of the silver paste layer is 0.15-0.30 mm.
[0023] Preferably, in step S5, the tantalum core immersed in the silver paste is dried at room temperature for 15 to 30 minutes until the surface of the silver paste layer is dry.
[0024] Preferably, in step S6, the tantalum core with the silver paste layer is cured at 180° C. to 210° C., and the sintering time is 20 to 40 minutes.
[0025] A chip-type tantalum capacitor prepared by the method.
[0026] The beneficial effects of the present invention are:
[0027] The present invention can effectively improve the interfacial bonding force between the graphite layer and the silver paste layer by using a surface treatment agent without changing the material formula of the graphite layer and the silver paste layer or improving the preparation process, thereby improving the performance stability and service life of the tantalum capacitor, and meeting the demand for high-performance tantalum capacitors in the field of electronic component manufacturing. Secondly, the implementation of this technical solution can avoid the use of special equipment or materials, reduce the manufacturing cost of tantalum capacitors, and meet the market demand for low-cost and high-performance tantalum capacitors. Finally, the present invention has a significant effect on improving the interfacial bonding force between the graphite layer and the silver paste layer, and can meet the demand for high interfacial bonding force in the field of tantalum capacitor manufacturing. Therefore, the method of the present invention has broad market application prospects and needs.
[0028] The present invention mainly solves the following technical problems: 1) how to improve the interface bonding force between the graphite layer and the silver paste layer without changing the material formula of the two layers or improving the preparation process; 2) how to reduce the manufacturing cost of tantalum capacitors without using special equipment or materials; 3) how to improve the interface bonding force between the graphite layer and the silver paste layer without affecting other properties of the tantalum capacitor, such as capacity and leakage current; 4) how to further improve the interface bonding force between the graphite layer and the silver paste layer to meet practical application requirements. DETAILED DESCRIPTION
[0029] The technical solution of the present invention is further described below, but the scope of protection claimed is not limited to the description.
[0030] Embodiment 1:
[0031] A method for preparing a chip tantalum capacitor comprises the following steps:
[0032] Step 1: Press tantalum metal powder into tantalum blocks and place the tantalum blocks on a 2×10 -3 Pa vacuum environment, sintering temperature 1390 ℃, sintering time 20min, the sintered tantalum block has a certain mechanical strength and a porous structure;
[0033] Step 2: The Ta formed on the surface of the sintered tantalum block by anodizing2 O 5 The dielectric oxide film is then deposited on the surface of the dielectric oxide film by thermal decomposition. 2 , we get MnO 2 layer, MnO 2 The layer serves as the cathode of the tantalum capacitor;
[0034] Step 3: MnO 2 The surface of the layer is coated with a graphite layer with a thickness of 0.1 mm to obtain a tantalum core, and then the tantalum core is immersed in a surface treatment agent for 1 min;
[0035] Step 4: Dry the tantalum core after impregnation with the surface treatment agent at room temperature for 10 minutes to remove excess solvent, and then place it in a blast drying oven for baking at 150°C for 30 minutes, so that the silane coupling agent can be firmly attached to the surface of the graphite layer;
[0036] Step 5: Impregnate a layer of silver paste on the treated graphite layer of the tantalum core to form a silver paste layer with a thickness of 0.15 mm. Due to the presence of the silane coupling agent, the interfacial bonding force between the graphite layer and the silver paste layer can be significantly improved. The tantalum core impregnated with the silver paste is dried at room temperature for 15 minutes until the surface of the silver paste layer is dry, and then cured so that the silver paste layer can be firmly bonded to the surface of the graphite layer, thereby improving the overall performance of the tantalum capacitor;
[0037] Step 6: The tantalum core with the silver paste layer is cured at 180°C for 20 minutes. After the preparation is completed, the capacitor can be tested and evaluated. The test content includes capacity, voltage resistance, etc. to evaluate the effect of surface treatment and the performance of tantalum capacitors.
[0038] The surface treatment agent comprises a mixture of a silane coupling agent, anhydrous ethanol and deionized water, wherein the volume ratio of the anhydrous ethanol to the deionized water is 1:1, and the surface treatment agent is hydrolyzed for 0.5h;
[0039] Silane coupling agents include γ-aminopropyl-triethoxysilane and γ-glycidyloxypropyl-trimethoxysilane.
[0040] The mass concentration of the silane coupling agent is 15%.
[0041] The method of Example 1 was used to produce a CAK45U-16-100 16V 100μF H-shell chip tantalum capacitor. The performance test results are shown in the following table.
[0042] Shear force(N) 78.8 76.1 73.9 75.7 72.6 ESR(Ω) 92 95 98 94 96 C(μF) 103 102 103 103 102 Id 3 2 2 3 2
[0043] Embodiment 2:
[0044] A method for preparing a chip tantalum capacitor comprises the following steps:
[0045] Step 1: Press tantalum metal powder into tantalum blocks and place the tantalum blocks on a 4×10 -3 The sintering is carried out in a vacuum environment of Pa, the sintering temperature is 1450℃, and the sintering time is 40min. The sintered tantalum block has a certain mechanical strength and a porous structure.
[0046] Step 2: Use anodization to form Ta on the surface of the sintered tantalum block 2 O 5 The dielectric oxide film is then deposited on the surface of the dielectric oxide film by thermal decomposition. 2 , we get MnO 2 layer, MnO 2 The layer serves as the cathode of the tantalum capacitor;
[0047] Step 3: MnO 2 The surface of the layer is coated with a graphite layer with a thickness of 0.2 mm to obtain a tantalum core, and then the tantalum core is immersed in a surface treatment agent for 10 minutes;
[0048] Step 4: Dry the tantalum core after impregnation with the surface treatment agent at room temperature for 30 minutes to remove excess solvent, and then place it in a blast drying oven at 200° C. for baking for 60 minutes, so that the silane coupling agent can be firmly attached to the surface of the graphite layer;
[0049] Step 5: A layer of silver paste is impregnated on the treated graphite layer of the tantalum core to form a silver paste layer with a thickness of 0.30 mm. Due to the presence of the silane coupling agent, the interfacial bonding force between the graphite layer and the silver paste layer can be significantly improved. The tantalum core impregnated with the silver paste is dried at room temperature for 30 minutes until the surface of the silver paste layer is dry, and then cured so that the silver paste layer can be firmly bonded to the surface of the graphite layer, thereby improving the overall performance of the tantalum capacitor;
[0050] Step 6: The tantalum core with the silver paste layer is cured at 210°C for 40 minutes. After the preparation is completed, the capacitor can be tested and evaluated. The test content includes capacity, voltage resistance, etc. to evaluate the effect of surface treatment and the performance of tantalum capacitors.
[0051] The surface treatment agent in step S3 is a silane coupling agent, including γ-methacryloxy-trimethoxysilane and vinyl trichlorosilane.
[0052] The surface treatment agent comprises a mixture of a silane coupling agent, anhydrous ethanol and deionized water, wherein the volume ratio of anhydrous ethanol to deionized water is 7:4, and the surface treatment agent is hydrolyzed for 1 hour;
[0053] Silane coupling agents include γ-methacryloxy-trimethoxysilane and vinyltrichlorosilane.
[0054] The mass concentration of the silane coupling agent is 25%.
[0055] The method of Example 2 was used to produce a CAK45U-16-100 16V 100μF H-shell chip tantalum capacitor. The performance test results are shown in the following table.
[0056] Shear force(N) 73.6 72.9 75.4 73.8 73.1 ESR(Ω) 111 115 115 110 106 C(μF) 102 103 103 103 103 Id 3 3 3 3 2
[0057] Embodiment 3:
[0058] A method for preparing a chip tantalum capacitor comprises the following steps:
[0059] Step 1: Press tantalum metal powder into tantalum blocks and place the tantalum blocks on a 3×10 -3 Pa vacuum environment, sintering temperature 1425 ℃, sintering time 30min, the sintered tantalum block has a certain mechanical strength and a porous structure;
[0060] Step 2: Use anodization to form Ta on the surface of the sintered tantalum block 2 O 5 The dielectric oxide film is then deposited on the surface of the dielectric oxide film by thermal decomposition. 2 , we get MnO 2 layer, MnO 2 The layer serves as the cathode of the tantalum capacitor;
[0061] Step 3: MnO 2 The surface of the layer is coated with a graphite layer with a thickness of 0.15 mm to obtain a tantalum core, and then the tantalum core is immersed in a surface treatment agent for 1 to 10 minutes;
[0062] Step 4: Dry the tantalum core after impregnation with the surface treatment agent at room temperature for 20 minutes to remove excess solvent, and then place it in a blast drying oven for baking at 180°C for 40 minutes, so that the silane coupling agent can be firmly attached to the surface of the graphite layer;
[0063] Step 5: A layer of silver paste is impregnated on the treated graphite layer of the tantalum core to form a silver paste layer with a thickness of 0.25 mm. Due to the presence of the silane coupling agent, the interfacial bonding force between the graphite layer and the silver paste layer can be significantly improved. The tantalum core impregnated with the silver paste is dried at room temperature for 23 minutes until the surface of the silver paste layer is dry, and then cured so that the silver paste layer can be firmly bonded to the surface of the graphite layer, thereby improving the overall performance of the tantalum capacitor;
[0064] Step 6: The tantalum core with the silver paste layer is cured at 196°C for 31 minutes. After the preparation is completed, the capacitor can be tested and evaluated. The test content includes capacity, voltage resistance, etc. to evaluate the effect of surface treatment and the performance of tantalum capacitors.
[0065] The surface treatment agent in step S3 is a silane coupling agent, including γ-aminopropyl-triethoxysilane and vinyl trichlorosilane.
[0066] The surface treatment agent includes a mixture of silane coupling agent, anhydrous ethanol and deionized water, the volume ratio of anhydrous ethanol to deionized water is 5:2, and the surface treatment agent is hydrolyzed for 0.8h;
[0067] Silane coupling agents include gamma-aminopropyl-triethoxysilane and vinyltrichlorosilane.
[0068] The mass concentration of the silane coupling agent is 18%.
[0069] The method of Example 3 was used to produce a CAK45U-16-100 16V 100μF H-shell chip tantalum capacitor. The performance test results are shown in the following table.
[0070] Shear force(N) 76.4 74.5 76.5 78.4 79.8 ESR(Ω) 99 97 95 93 94 C(μF) 103 102 103 102 103 Id 3 3 2 3 2
[0071] Comparative Example 1:
[0072] The performance test results of the CAK45U-16-100 16V 100μF H-shell tantalum capacitor produced using existing technology are shown in the following table.
[0073] Shear force(N) 62.1 61.5 55.3 58.6 56.1 ESR(Ω) 109 112 115 106 108 C(μF) 103 103 102 102 103 <![CDATA[I d ]]> 2 3 3 3 2
[0074] The test results of Examples 1-3 and Comparative Example 1 show that the interface bonding force between the graphite layer and the silver paste layer of the surface-treated tantalum capacitor is increased by up to 31.3%, and the capacity and leakage current of the tantalum capacitor do not change significantly.
Claims
1. A method for preparing a chip tantalum capacitor, It is characterized in that The following steps are involved: Step 1: Pressing tantalum metal powder into tantalum blocks, and sintering the tantalum blocks in a vacuum environment; Step 2: Form an oxide film on the surface of the sintered tantalum block, and then deposit MnO on the surface of the oxide film. 2 , we get MnO 2 layer; Step 3: MnO 2 The surface of the layer is covered with a graphite layer to obtain a tantalum core, and then the tantalum core is immersed in a surface treatment agent; Step 4: Drying and baking the tantalum core after being impregnated with the surface treatment agent; Step 5: impregnate a layer of silver paste on the treated graphite layer of the tantalum core to form a silver paste layer; Step 6: Perform curing treatment and test and evaluate the capacitor after preparation.
2. A method for preparing a chip tantalum capacitor as claimed in claim 1, Features: In step S3, the surface treatment agent includes a mixture of silane coupling agent, anhydrous ethanol and deionized water, the volume ratio of anhydrous ethanol to deionized water is 4-7:4-1, and the surface treatment agent is hydrolyzed for 0.5h-1h; The silane coupling agent includes one or more of γ-aminopropyl-triethoxysilane, γ-glycidyloxypropyl-trimethoxysilane, γ-methacryloxy-trimethoxysilane, and vinyltrichlorosilane.
3. A method for preparing a chip tantalum capacitor as claimed in claim 2, Features: The mass concentration of the one or more silane coupling agents is 15% to 25%.
4. The method for preparing a chip tantalum capacitor according to claim 1, Features: In step S1, the tantalum block is 2×10 -3 Pa~4×10 -3 Sintering is carried out in a vacuum environment of Pa; In step S2, an anodic oxidation method is used to form Ta on the surface of the sintered tantalum block. 2 O 5 The dielectric oxide film is then thermally decomposed on Ta 2 O 5 MnO deposition on the surface of dielectric oxide film 2 .
5. The method for preparing a chip tantalum capacitor according to claim 1, Features: The immersion time in step S3 is 1 to 10 minutes.
6. The method for preparing a chip tantalum capacitor according to claim 1, Features: In the step S4, the tantalum core impregnated with the surface treatment agent is dried at room temperature for 10 to 30 minutes, and then baked at 150° C. to 200° C. for 30 to 60 minutes.
7. The method for preparing a chip tantalum capacitor according to claim 1, Features: The thickness of the silver paste layer in step S5 is 0.15-0.30 mm.
8. The method for preparing a chip tantalum capacitor according to claim 1, Features: In the step S5, the tantalum core immersed in the silver paste is dried at room temperature for 15 to 30 minutes until the surface of the silver paste layer is dry.
9. The method for preparing a chip tantalum capacitor according to claim 1, Features: In the step S6, the tantalum core with the silver paste layer is cured at 180° C. to 210° C., and the sintering time is 20 to 40 minutes.
10. A chip tantalum capacitor prepared by the method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Polymer chip tantalum capacitor silver paste and preparation method thereof
CN116013576A
Organic chip type solid tantalum electrolytic capacitor and preparation method thereof
CN117995561A
Cited By
High-specific-volume chip tantalum capacitor and preparation method thereof