Process for synthesizing indium arsenide epitaxial thin film wafer by utilizing arsenic tribromide

By reacting arsenic tribromide with high pressure hydrogen on an indium antimonide substrate to generate an indium arsenide epitaxial thin film wafer, the problems of high production costs and insufficient film thickness in the existing methods are solved, and efficient and low-cost arsenic is achieved Indium film is prepared with a thickness of 50μm.

CN119008381AActive Publication Date: 2024-11-22SUZHOU HENGWEI OPTOELECTRONICS TECHNOLOGY CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411077386.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-22
Estimated Expiration
2044-08-07

AI Technical Summary

Technical Problem

The existing method of epitaxially growing indium arsenide thin film wafers on indium antimonide substrates has high production cost, low reaction efficiency, and the generated indium arsenide thin film is thin, only about 10 μm.

Method used

Arsenic tribromide and high-pressure hydrogen react on indium antimonide substrate to form an indium arsenide epitaxial thin film wafer. The reaction temperature and pressure are controlled through heating elements to improve the reaction efficiency, and liquid arsenic tribromide is used as raw material to reduce production costs .

Benefits of technology

The reaction time is shortened, the reaction temperature is reduced, the reaction efficiency is improved, the thickness of the indium arsenide film is increased to 50 μm, the dependence on high-purity arsenic is reduced, and the production cost is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008381A_ABST
    Figure CN119008381A_ABST
Patent Text Reader

Abstract

The invention discloses a process for synthesizing an indium arsenide epitaxial thin film wafer by utilizing arsenic tribromide, and belongs to the technical field of semiconductor materials. The process comprises the following steps: (1) replacing air in a reaction tube with hydrogen; placing the indium antimonide substrate in a reaction tube, and uniformly placing indium particles with small particle sizes on the surface of the indium antimonide substrate; (2) the indium antimonide substrate and the indium particles are heated, so that the indium particles are molten and are uniformly attached to the surface of the indium antimonide substrate; (3) heating the liquid arsenic tribromide storage tank to gasify the liquid arsenic tribromide, and introducing the gasified liquid arsenic tribromide into the reaction tube through hydrogen; (4) the reaction tube is heated, so that the small-particle-size indium particles, the arsenic tribromide and the hydrogen react, and indium arsenide is generated on the indium antimonide substrate; and (5) cooling to obtain an indium arsenide epitaxial thin film wafer finished product. The liquid arsenic tribromide is adopted as the raw material, so that the dependence on the upstream raw material high-purity arsenic is reduced, and the production cost is reduced; and the thickness of the prepared indium arsenide epitaxial thin film wafer is also obviously improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of semiconductor materials, in particular to a process for synthesizing indium arsenide epitaxial thin film wafers using arsenic tribromide. Background Art

[0002] The molecular formula of indium antimonide is InSb, and the molecular weight is 236.578. It is a compound semiconductor with metallic luster, sphalerite structure, direct transition type energy band structure, melting point 525℃, and low dislocation density of single crystal material. The band gap width at room temperature is 0.18 electron volts, which is an ultra-narrow band gap semiconductor material. The corresponding electro-stimulated light wavelength is 5.3 microns, which is just suitable for the detection wavelength requirements of medium-wave infrared radiation signals. It is an infrared detector material with excellent performance. The chemical formula of indium arsenide is InAs, which is a compound semiconductor material. It is a silver-gray solid at room temperature, has a sphalerite crystal structure, a lattice constant of 0.6058nm, a direct transition energy band structure, and a band gap width (300K) of 0.45eV. It has the characteristics of high saturated electron drift velocity, high photoelectric conversion efficiency, and ultra-narrow band gap width. It is an ideal material for manufacturing Hall devices and magnetoresistive devices, and is also widely used in the field of infrared optical devices.

[0003] Indium antimonide and indium arsenide are both semiconductor materials with similar energy band structures and similar bandgap widths (0.18eV and 0.45eV respectively). They both have the characteristics of high saturated electron drift velocity, high photoelectric conversion efficiency, and ultra-narrow bandgap width. They are both new generation infrared semiconductor basic materials. Epitaxial growth of indium arsenide thin film wafers on indium antimonide substrates can obtain semiconductor composite materials with specific properties. The existing methods for epitaxial growth of indium arsenide thin film wafers on indium antimonide substrates mostly use high-purity indium as raw material, which has high production costs and low reaction efficiency. In addition, the generated indium arsenide film is relatively thin, only about 10μm. Summary of the invention

[0004] Based on the above technical problems, the present invention proposes a process for synthesizing indium arsenide epitaxial thin film wafers using arsenic tribromide.

[0005] The technical solution adopted by the present invention is:

[0006] A process for synthesizing indium arsenide epitaxial thin film wafers using arsenic tribromide, which uses a device for synthesizing indium arsenide epitaxial thin film wafers using arsenic tribromide, the device comprising a reaction tube, a high-pressure hydrogen storage tank and a liquid arsenic tribromide storage tank;

[0007] The high-pressure hydrogen storage tank is connected to the inlet end of the reaction tube through a hydrogen delivery pipeline, and the liquid arsenic tribromide storage tank is connected to the hydrogen delivery pipeline through an arsenic tribromide gas delivery pipeline; a first heating element is arranged on the outer side of the liquid arsenic tribromide storage tank;

[0008] A second heating element is arranged outside the reaction tube, a bracket is arranged inside the reaction tube, a third heating element is arranged at the bracket, and an outlet end of the reaction tube is connected to an exhaust gas output pipeline;

[0009] The process includes the following steps:

[0010] (1) hydrogen in a high-pressure hydrogen storage tank is transported to a reaction tube through a hydrogen transport pipeline to completely replace the air in the reaction tube; an indium antimonide substrate is placed on a bracket, and small-diameter indium particles are placed on the surface of the indium antimonide substrate;

[0011] (2) using a third heating element to heat the indium antimonide substrate and the indium particles, so that the indium particles are melted and uniformly adhere to the surface of the indium antimonide substrate;

[0012] (3) heating the liquid arsenic tribromide storage tank by a first heating element so that the liquid arsenic tribromide in the liquid arsenic tribromide storage tank is vaporized; the vaporized arsenic tribromide is introduced into the reaction tube by hydrogen;

[0013] (4) heating the reaction tube to 400-450° C. by a second heating element, so that the small-size indium particles, arsenic tribromide and hydrogen react to generate indium arsenide on the indium antimonide substrate; the hydrogen bromide generated by the reaction is discharged through an exhaust gas output pipeline;

[0014] (5) After the reaction is completed, hydrogen gas at room temperature is continuously introduced into the reaction tube, and the tube is cooled to room temperature to obtain a finished indium arsenide epitaxial thin film wafer.

[0015] Preferably, the reaction tube is arranged horizontally, and the inlet end and the outlet end of the reaction tube are respectively arranged at two ends of the reaction tube; the bracket is arranged at the middle position of the bottom wall of the reaction tube.

[0016] Preferably, a heat insulating material is arranged on the outside of the reaction tube, and the heat insulating material is made of ceramic fiber; the second heating element is arranged between the heat insulating material and the outer wall of the reaction tube.

[0017] Preferably, in step (1): the indium antimonide substrate is placed in a quartz boat, and the small-diameter indium particles are coated on the upper surface of the indium antimonide substrate.

[0018] Preferably, the particle size of the small-size indium particles is 0.8-1 micrometer, and the amount of the small-size indium particles used is 50-60 micrograms.

[0019] Preferably, in step (2): the third heating element is controlled to heat to 200-250°C.

[0020] Preferably, in step (3): the arsenic tribromide storage tank is heated to 220-250°C.

[0021] Preferably, in step (4), while heating the reaction tube, the system pressure in the reaction tube needs to be maintained at 1-1.2 MPa; and the reaction is continued at 400-450° C. for 2-3 hours.

[0022] Preferably, in step (4): the waste gas output pipeline is also connected to a waste liquid discharge pipe and a waste gas discharge pipe respectively, the waste liquid discharge pipe is connected to a waste liquid storage tank, and the waste gas discharge pipe is connected to a waste gas treatment system;

[0023] The waste gas in the reaction tube is discharged through the waste gas output pipe. During the discharge process, the arsenic tribromide in the waste gas is condensed into liquid and refluxed to the waste liquid storage tank through the waste liquid discharge pipe for storage. The hydrogen bromide gas and hydrogen in the waste gas are transported to the waste gas treatment system through the waste gas discharge pipe for incineration or reuse.

[0024] Preferably, in step (5): the thickness of the indium arsenide epitaxial thin film wafer is 50-55 μm.

[0025] The beneficial technical effects of the present invention are:

[0026] The present invention uses arsenic tribromide mixed with hydrogen to synthesize an indium arsenide epitaxial thin film wafer on the surface of an indium antimonide substrate with molten high-purity indium, which greatly shortens the reaction time, reduces the reaction temperature, and improves the reaction efficiency; and liquid arsenic tribromide is used as a raw material, and the purification difficulty of liquid arsenic tribromide is much lower than that of high-purity arsenic, and its price is also much lower than that of high-purity arsenic. Therefore, using arsenic tribromide as a raw material not only reduces the dependence on upstream raw material high-purity arsenic, but also reduces the production cost. The process of the present invention can also increase the thickness of the prepared indium arsenide epitaxial thin film wafer. After observation and testing, the thickness of the indium arsenide epitaxial thin film wafer synthesized by the present invention reaches 50μm, which is significantly improved compared with the thinner indium arsenide film of about 10μm synthesized by the conventional method. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 The process flow chart of the present invention for synthesizing indium arsenide epitaxial thin film wafers using arsenic tribromide;

[0028] Figure 2 This is a schematic diagram of the structure principle of the device for synthesizing indium arsenide epitaxial thin film wafers using arsenic tribromide in the present invention;

[0029] Figure 3 This is a micrograph of the indium arsenide epitaxial thin film wafer prepared in Example 1 of the present invention;

[0030] Figure 4 This is an XRD scan of the indium arsenide epitaxial thin film wafer prepared in Example 1 of the present invention;

[0031] Figure 5 This is the PL room temperature spectrum of the InAs epitaxial thin film wafer prepared in Example 1 of the present invention.

[0032] In the figure: 1-reaction tube, 2-high-pressure hydrogen storage tank, 3-liquid arsenic tribromide storage tank, 4-hydrogen delivery pipeline, 5-boosting pump, 6-arsenic tribromide gas delivery pipeline, 7-first heating element, 8-second heating element, 9-ceramic fiber sheet, 10-bracket, 11-waste gas output pipeline, 12-waste liquid discharge pipe, 13-waste gas discharge pipe, 14-waste liquid storage tank, 15-third heating element. DETAILED DESCRIPTION

[0033] Epitaxial growth of indium arsenide thin film wafers on indium antimonide substrates can produce semiconductor composite materials with specific properties (such as increasing the transition wavelength to 2.3 μm). Based on this, the present invention innovatively proposes a process for synthesizing indium arsenide epitaxial thin film wafers using arsenic tribromide, which places a quartz boat containing an indium antimonide substrate in the middle of a reaction tube, uses high-purity hydrogen to carry gaseous arsenic tribromide, and reacts with a thin layer of high-purity indium on the indium antimonide substrate to synthesize an indium arsenide epitaxial thin film product.

[0034] The present invention will be further described below in conjunction with specific embodiments.

[0035] Example 1

[0036] A process for synthesizing indium arsenide epitaxial thin film wafers using arsenic tribromide, and a device for synthesizing indium arsenide epitaxial thin film wafers using arsenic tribromide, such as Figure 2 As shown, the device includes a reaction tube 1, a high-pressure hydrogen storage tank 2 and a liquid arsenic tribromide storage tank 3. The high-pressure hydrogen storage tank 2 is connected to the inlet end of the reaction tube 1 through a hydrogen delivery pipeline 4, and a pressure pump 5 is arranged on the hydrogen delivery pipeline 4. The liquid arsenic tribromide storage tank 3 is connected to the hydrogen delivery pipeline 4 through an arsenic tribromide gas delivery pipeline 6. A first heating element 7 is arranged on the outside of the liquid arsenic tribromide storage tank 3. A second heating element 8 is arranged on the outside of the reaction tube 1, and a heat insulation material is arranged on the outside of the reaction tube 1. The heat insulation material adopts a ceramic fiber sheet 9 to isolate high temperature. The second heating element 8 is arranged between the heat insulation material and the outer wall of the reaction tube. A bracket 10 is arranged inside the reaction tube 1, and the cross section of the bracket 10 is T-shaped. The bracket 10 is arranged at the middle position of the bottom wall of the reaction tube 1, and a third heating element 15 is arranged at the bracket 10. The reaction tube 1 is arranged horizontally, and the inlet and outlet of the reaction tube 1 are respectively arranged at both ends of the reaction tube 1, and the outlet of the reaction tube 1 is connected to the exhaust gas output pipe 11. The exhaust gas output pipe 11 is also connected to the waste liquid discharge pipe 12 and the exhaust gas discharge pipe 13 respectively, the waste liquid discharge pipe 12 is connected to the waste liquid storage tank 14, and the exhaust gas discharge pipe 13 is connected to the exhaust gas treatment system.

[0037] like Figure 1 As shown, the process includes the following steps:

[0038] (1) The hydrogen in the high-pressure hydrogen storage tank 2 is transported to the reaction tube 1 through the hydrogen delivery pipeline 4 to completely replace the air in the reaction tube 1. The indium antimonide substrate is placed in a quartz boat, and the quartz boat is placed on the bracket 10. High-purity small-particle indium particles are quickly placed on the upper surface of the indium antimonide substrate. The particle size of the small-particle indium particles is 1 micron, and the amount of the small-particle indium particles is 50 micrograms.

[0039] (2) The reaction tube 1 is heated by the third heating element 15, and is first heated to about 250° C., so that the high-purity small-diameter indium particles are completely melted and attached to the surface of the indium antimonide substrate.

[0040] (3) The liquid arsenic tribromide storage tank 3 is heated by the first heating element 7, and the arsenic tribromide storage tank is slowly heated to 220° C., so that the liquid arsenic tribromide in the liquid arsenic tribromide storage tank is vaporized. The vaporized arsenic tribromide is introduced into the reaction tube 1 by hydrogen.

[0041] (4) The reaction tube is further heated to 400°C by the second heating element 8, and the system pressure in the reaction tube is maintained at 1 MPa. At this temperature and pressure, the molten small-sized indium particles, arsenic tribromide and hydrogen continue to undergo the following disproportionate chemical reaction on the surface of the indium antimonide substrate, generating indium arsenide on the indium antimonide substrate. The chemical reaction formula is as follows:

[0042] 2AsBr 3 +3H 2 +2In=2InAs+6HBr;

[0043] The reaction time is 2.5 hours. The hydrogen bromide produced by the reaction is discharged through the waste gas output pipe 11. During the discharge process, the arsenic tribromide in the waste gas is condensed into liquid and refluxed to the waste liquid storage tank 14 through the waste liquid discharge pipe 12 for storage, and the hydrogen bromide gas and hydrogen in the waste gas are transported to the waste gas treatment system through the waste gas discharge pipe 13 for incineration or reuse.

[0044] (5) After the reaction is completed, hydrogen gas at room temperature is continuously introduced into the reaction tube 1, and the reaction tube is cooled to room temperature. The product is taken out to obtain a finished indium arsenide epitaxial thin film wafer.

[0045] Figure 3 This is a micrograph of the InAs epitaxial thin film wafer prepared in Example 1 of the present invention. It can be seen from the figure that the thickness of the InAs epitaxial thin film wafer synthesized in the present invention is 50 μm. Figure 4 This is an XRD scan of the indium arsenide epitaxial thin film wafer prepared in Example 1 of the present invention. Figure 4 The crystal orientation distribution of the InAs epitaxial thin film wafer is shown, with the (111) crystal orientation being the most concentrated. Figure 5 This is the PL room temperature spectrum of the InAs epitaxial thin film wafer prepared in Example 1 of the present invention. Figure 5It shows that the characteristic spectrum of 2.3μm wavelength unique to indium arsenide appears in the wafer where the thin film is formed.

[0046] Example 2

[0047] A process for synthesizing indium arsenide epitaxial thin film wafers using arsenic tribromide, and a device for synthesizing indium arsenide epitaxial thin film wafers using arsenic tribromide, the structure of which is the same as that of Example 1. The process comprises the following steps:

[0048] (1) The hydrogen in the high-pressure hydrogen storage tank 2 is transported to the reaction tube 1 through the hydrogen delivery pipeline 4 to completely replace the air in the reaction tube 1. The indium antimonide substrate is placed in a quartz boat, and the quartz boat is placed on a bracket. High-purity small-particle indium particles are quickly placed on the upper surface of the indium antimonide substrate. The particle size of the small-particle indium particles is 0.8 microns, and the amount of the small-particle indium particles is 60 micrograms.

[0049] (2) The reaction tube 1 is heated by the third heating element 15, and is first heated to about 200° C., so that the high-purity small-diameter indium particles are completely melted and attached to the surface of the indium antimonide substrate.

[0050] (3) The liquid arsenic tribromide storage tank 3 is heated by the first heating element 7, and the arsenic tribromide storage tank is slowly heated to 250° C., so that the liquid arsenic tribromide in the liquid arsenic tribromide storage tank is vaporized. The vaporized arsenic tribromide is introduced into the reaction tube 1 by hydrogen.

[0051] (4) The reaction tube is further heated to 450°C by the second heating element 8, and the system pressure in the reaction tube is maintained at 1.2 MPa. At this temperature and pressure, the molten small-sized indium particles, arsenic tribromide and hydrogen continue to undergo the following disproportionate chemical reaction on the surface of the indium antimonide substrate, generating indium arsenide on the indium antimonide substrate. The chemical reaction formula is as follows:

[0052] 2AsBr 3 +3H 2 +2In=2InAs+6HBr;

[0053] The reaction lasts for 2 hours. The hydrogen bromide produced by the reaction is discharged through the waste gas output pipe 11. During the discharge process, the arsenic tribromide in the waste gas is condensed into a liquid state and refluxed to the waste liquid storage tank 14 through the waste liquid discharge pipe 12 for storage, and the hydrogen bromide gas and hydrogen in the waste gas are transported to the waste gas treatment system through the waste gas discharge pipe 13 for incineration or reuse.

[0054] (5) After the reaction is completed, hydrogen gas at room temperature is continuously introduced into the reaction tube 1, and the reaction tube is cooled to room temperature. The product is taken out to obtain a finished indium arsenide epitaxial thin film wafer.

[0055] Example 3

[0056] A process for synthesizing indium arsenide epitaxial thin film wafers using arsenic tribromide, and a device for synthesizing indium arsenide epitaxial thin film wafers using arsenic tribromide, the structure of which is the same as that of Example 1. The process comprises the following steps:

[0057] (1) The hydrogen in the high-pressure hydrogen storage tank 2 is transported to the reaction tube 1 through the hydrogen delivery pipeline 4 to completely replace the air in the reaction tube 1. The indium antimonide substrate is placed in a quartz boat, and the quartz boat is placed on a bracket. High-purity small-particle indium particles are quickly placed on the upper surface of the indium antimonide substrate. The particle size of the small-particle indium particles is 0.9 microns, and the amount of the small-particle indium particles is 55 micrograms.

[0058] (2) The reaction tube 1 is heated by the third heating element 8, and is first heated to about 220° C., so that the high-purity small-diameter indium particles are completely melted and attached to the surface of the indium antimonide substrate.

[0059] (3) The liquid arsenic tribromide storage tank 3 is heated by the first heating element 7, and the arsenic tribromide storage tank is slowly heated to 230° C., so that the liquid arsenic tribromide in the liquid arsenic tribromide storage tank is vaporized. The vaporized arsenic tribromide is introduced into the reaction tube 1 by hydrogen.

[0060] (4) The reaction tube is further heated to 430°C by the second heating element 8, and the system pressure in the reaction tube is maintained at 1 MPa. At this temperature and pressure, the molten small-sized indium particles, arsenic tribromide and hydrogen continue to undergo the following disproportionate chemical reaction on the surface of the indium antimonide substrate, generating indium arsenide on the indium antimonide substrate. The chemical reaction formula is as follows:

[0061] 2AsBr 3 +3H 2 +2In=2InAs+6HBr;

[0062] The reaction lasts for 3 hours. The hydrogen bromide produced by the reaction is discharged through the waste gas output pipe 11. During the discharge process, the arsenic tribromide in the waste gas is condensed into a liquid state and refluxed to the waste liquid storage tank 14 through the waste liquid discharge pipe 12 for storage, and the hydrogen bromide gas and hydrogen in the waste gas are transported to the waste gas treatment system through the waste gas discharge pipe 13 for incineration or reuse.

[0063] (5) After the reaction is completed, hydrogen gas at room temperature is continuously introduced into the reaction tube 1, and the reaction tube is cooled to room temperature. The product is taken out to obtain a finished indium arsenide epitaxial thin film wafer.

[0064] The parts not mentioned in the above methods can be realized by adopting or drawing on existing technologies.

[0065] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A process for synthesizing indium arsenide epitaxial thin film wafers using arsenic tribromide, characterized in that: A device for synthesizing indium arsenide epitaxial thin film wafers using arsenic tribromide, the device comprising a reaction tube, a high-pressure hydrogen storage tank and a liquid arsenic tribromide storage tank; The high-pressure hydrogen storage tank is connected to the inlet end of the reaction tube through a hydrogen delivery pipeline, and the liquid arsenic tribromide storage tank is connected to the hydrogen delivery pipeline through an arsenic tribromide gas delivery pipeline; a first heating element is arranged on the outer side of the liquid arsenic tribromide storage tank; A second heating element is arranged outside the reaction tube, a bracket is arranged inside the reaction tube, a third heating element is arranged at the bracket, and an outlet end of the reaction tube is connected to an exhaust gas output pipeline; The process includes the following steps: (1) hydrogen in a high-pressure hydrogen storage tank is transported to a reaction tube through a hydrogen transport pipeline to completely replace the air in the reaction tube; an indium antimonide substrate is placed on a bracket, and indium particles are placed on the surface of the indium antimonide substrate; (2) using a third heating element to heat the indium antimonide substrate and the indium particles, so that the indium particles are melted and uniformly adhere to the surface of the indium antimonide substrate; (3) heating the liquid arsenic tribromide storage tank by a first heating element so that the liquid arsenic tribromide in the liquid arsenic tribromide storage tank is vaporized; the vaporized arsenic tribromide is introduced into the reaction tube by hydrogen; (4) heating the reaction tube to 400-450° C. by a second heating element, so that the indium particles, arsenic tribromide and hydrogen react to form indium arsenide on the indium antimonide substrate; the hydrogen bromide generated by the reaction is discharged through an exhaust gas output pipeline; (5) After the reaction is completed, hydrogen gas at room temperature is continuously introduced into the reaction tube, and the tube is cooled to room temperature to obtain a finished indium arsenide epitaxial thin film wafer.

2. The process for synthesizing indium arsenide epitaxial thin film wafers using arsenic tribromide according to claim 1, characterized in that: The reaction tube is arranged horizontally, and the inlet end and the outlet end of the reaction tube are respectively arranged at the two ends of the reaction tube; the bracket is arranged at the middle position of the bottom wall of the reaction tube.

3. The process for synthesizing indium arsenide epitaxial thin film wafers using arsenic tribromide according to claim 1, characterized in that: A heat insulating material is arranged on the outside of the reaction tube, and the heat insulating material is made of ceramic fiber; the second heating element is arranged between the heat insulating material and the outer wall of the reaction tube.

4. A process for synthesizing indium arsenide epitaxial thin film wafers using arsenic tribromide according to claim 1, characterized in that: In step (1): the indium antimonide substrate is placed in a quartz boat, and the indium particles are smeared on the upper surface of the indium antimonide substrate.

5. The process for synthesizing indium arsenide epitaxial thin film wafers using arsenic tribromide according to claim 4, characterized in that: The particle size of the indium particles is 0.8-1 micrometer, and the dosage of the indium particles is 50-60 micrograms.

6. A process for synthesizing indium arsenide epitaxial thin film wafers using arsenic tribromide according to claim 1, characterized in that: In step (2): the third heating element is controlled to heat to 200-250°C.

7. The process for synthesizing indium arsenide epitaxial thin film wafers using arsenic tribromide according to claim 1, characterized in that: In step (3): the arsenic tribromide storage tank is controlled to be heated to 220-250°C.

8. The process for synthesizing indium arsenide epitaxial thin film wafers using arsenic tribromide according to claim 1, characterized in that: In step (4): while heating the reaction tube, the system pressure in the reaction tube needs to be maintained at 1-1.2 MPa; and the reaction is continued at 400-450° C. for 2-3 hours.

9. The process for synthesizing indium arsenide epitaxial thin film wafers using arsenic tribromide according to claim 1, characterized in that: In step (4): the exhaust gas output pipeline is also connected to the waste liquid discharge pipe and the exhaust gas discharge pipe respectively, the waste liquid discharge pipe is connected to the waste liquid storage tank, and the exhaust gas discharge pipe is connected to the exhaust gas treatment system; The waste gas in the reaction tube is discharged through the waste gas output pipe. During the discharge process, the arsenic tribromide in the waste gas is condensed into liquid and refluxed to the waste liquid storage tank through the waste liquid discharge pipe for storage. The hydrogen bromide gas and hydrogen in the waste gas are transported to the waste gas treatment system through the waste gas discharge pipe for incineration or reuse.

10. The process for synthesizing indium arsenide epitaxial thin film wafers using arsenic tribromide according to claim 1, characterized in that: In step (5): the thickness of the indium arsenide epitaxial thin film wafer is 50-55 μm.

Citation Information

Patent Citations

  • Method for growing InAsxSb1-x film on gallium antimonide substrate

    CN101463499A

  • Preparation method and device of indium arsenide thin film material

    CN106783549A

  • Epitaxial layer structure of indium arsenide thin film, Hall device and preparation method

    CN115295719A

  • Production process for synthesizing indium phosphide epitaxial film wafer by using phosphorus trichloride

    CN116479529A

  • Devices Including Metal-Silicon Contacts Using Indium Arsenide Films and Apparatus and Methods