Chamber cleaning method
The multi-step plasma etching method removes organic polymers, inorganic deposits and metal deposition by-products in the chamber, solving the problem of difficulty in restoring the chamber environment and improving the consistency of the etching process and product yield.
Patent Information
- Application Number
- CN202411111158.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-22
AI Technical Summary
The prior art cannot effectively restore the chamber environment, resulting in poor consistency and repeatability of plasma etching processes, affecting product yield.
Using a multi-step plasma etching method, including removing organic polymers, inorganic deposits and metal deposition by-products, and gradually removing different types of by-products in the chamber through different gas combinations and power configurations, ensuring complete recovery of the chamber environment .
The comprehensive recovery of the chamber environment is achieved, the stability and consistency of the etching rate are improved, and the product yield is improved.
Smart Images

Figure CN119008386A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor manufacturing, and in particular to a chamber cleaning method. Background Art
[0002] As semiconductor manufacturing technology continues to develop, transistor density has doubled, and the industry has higher and higher requirements for the size, performance, and power consumption of electronic products, especially etching stability, which has an important impact on product yield. The importance of chamber environment to the consistency and repeatability of feature size etching between wafers has gradually become apparent. Changes in chamber environment have always been considered an important cause of process drift.
[0003] Plasma etching plays an extremely important role in the semiconductor manufacturing process. Plasma contains a large number of active particles such as electrons, ions, excited atoms, molecules and free radicals. These active particles interact with the wafer to produce various physical and chemical changes, so that the etching of the wafer can be precisely controlled. However, with the increase in the number of process wafers / hours, the etching byproducts (mainly including inorganic polymers such as silicon-based and silicon-based products, metal byproducts and organic polymers such as fluorine-containing and carbon-containing products) deposited on the surface of the components exposed to the plasma environment in the process chamber will continue to accumulate, resulting in the chamber environment between wafers in the continuous processing process. The recombination rate of active particles in the plasma at the chamber wall has also changed accordingly, resulting in changes in the chemical environment in the plasma, which is ultimately manifested in the process results, such as feature size, etching rate, etching uniformity, etching morphology, etching selectivity, etc., causing the drift of the process results.
[0004] At present, for capacitively coupled plasma (CCP) equipment, the method for cleaning polymer accumulation during the etching process is to perform a waferless auto dry cleaning (WLDC) process on the CCP equipment after each wafer is processed. This process uses a plasma formed by O2 with a large flow rate (e.g., 800sccm-1500sccm) to remove organic polymers. However, this method has weak cleaning ability and cannot completely restore the chamber environment. Figure 1 As shown, when the number of wafers processed by the existing method reaches a certain number or the process time reaches a certain length (for example, the moment corresponding to straight line A), the etching rate (ER) will gradually decrease due to the accumulation of etching by-products, and will drop below the straight line B corresponding to the lowest limit (Low limit), which not only causes the etching rate to fail to meet the requirements, but also leads to poor process consistency and repeatability, thereby affecting the product yield. Summary of the invention
[0005] The present invention aims to solve at least one of the technical problems existing in the prior art and proposes a chamber cleaning method, which can solve the problem that the prior art cannot completely restore the chamber environment, resulting in poor process consistency and repeatability, thereby affecting product yield.
[0006] To achieve the purpose of the present invention, a chamber cleaning method is provided, comprising: a first plasma etching step, and at least one of a second plasma etching step and a third plasma etching step; wherein:
[0007] The first plasma etching step is used to remove organic polymers on the surface in contact with the plasma in the process chamber;
[0008] The second plasma etching step is used to remove at least one of inorganic deposits on the surface of the designated component in the process chamber that contacts the plasma and organic polymers in the pore structure;
[0009] The third plasma etching step is used to remove metal deposition byproducts on the surface in contact with the plasma in the process chamber.
[0010] In some embodiments, in the first plasma etching step, plasma etching is performed using a first gas combination;
[0011] The first gas combination includes O2 and CF4.
[0012] In some embodiments, the flow rate of CF4 is 5‰ to 10‰ of the flow rate of O2.
[0013] In some embodiments, the flow rate of O2 is greater than or equal to 1500 sccm and less than or equal to 2000 sccm;
[0014] The flow rate of CF4 is greater than or equal to 5 sccm and less than or equal to 20 sccm.
[0015] In some embodiments, the first plasma etching step uses a chamber pressure greater than that of the second plasma etching step.
[0016] In some embodiments, the chamber pressure used in the second plasma etching step is greater than or equal to 45 mT and less than or equal to 60 mT.
[0017] In some embodiments, in the second plasma etching step, the upper DC power supply, the lower low-frequency RF power supply, and the lower high-frequency RF power supply are turned on;
[0018] The power output by the upper DC power supply in the second plasma etching step is greater than or equal to 300 W and less than or equal to 400 W;
[0019] The power outputted by the radio frequency power supply at high frequency in the second plasma etching step is greater than or equal to 1300 W and less than or equal to 1500 W;
[0020] The power output by the low-frequency RF power supply in the second plasma etching step is greater than or equal to 1500W and less than or equal to 1700W.
[0021] In some embodiments, in the second plasma etching step, plasma etching is performed using a second gas combination;
[0022] The second gas combination includes O2, a carbon-fluorine gas and a first inert gas.
[0023] In some embodiments, the fluorocarbon gas includes at least one of C4F8 and C4F6.
[0024] In some embodiments, the ratio of the flow rate of the fluorocarbon gas to the flow rate of O2 is greater than or equal to 2 and less than or equal to 3.
[0025] In some embodiments, the flow rate of O2 is greater than or equal to 20 sccm and less than or equal to 30 sccm;
[0026] The flow rate of the fluorocarbon gas is greater than or equal to 40 sccm and less than or equal to 60 sccm.
[0027] In some embodiments, the third plasma etching step includes:
[0028] In a first sub-etching step, a plasma formed by a third gas combination is used to perform a reduction reaction on the metal deposition byproduct;
[0029] In the second sub-etching step, the plasma formed by the fourth gas combination is used to physically bombard the products generated by the reduction reaction, so that the bombarded products are discharged from the chamber along with the gas flow.
[0030] In some embodiments, the third gas combination includes H 2 and a second inert gas.
[0031] In some embodiments, a ratio of a flow rate of the second inert gas to a flow rate of H2 is greater than or equal to 4 and less than or equal to 7.
[0032] In some embodiments, the flow rate of the second inert gas is greater than or equal to 250 sccm and less than or equal to 350 sccm;
[0033] The flow rate of H2 is greater than or equal to 40 sccm and less than or equal to 60 sccm.
[0034] In some embodiments, in the first sub-etching step, the high frequency lower RF power supply is turned on, and the upper DC power supply and the low frequency lower RF power supply are turned off;
[0035] The power output by the RF power supply at the high frequency in the first sub-etching step is less than the power output by the RF power supply at the high frequency in the second sub-etching step.
[0036] In some embodiments, the power output by the RF power supply at the high frequency in the first sub-etching step is greater than or equal to 700 W and less than or equal to 800 W.
[0037] In some embodiments, in the second sub-etching step, the upper DC power supply, the low-frequency lower RF power supply, and the high-frequency lower RF power supply are turned on;
[0038] The sum of the power output by the RF power supply at high frequency and the power output by the RF power supply at low frequency in the second sub-etching step is greater than the sum of the power output by the RF power supply at high frequency and the power output by the RF power supply at low frequency in the first plasma etching step.
[0039] In some embodiments, the power output by the RF power supply at high frequency in the second sub-etching step is greater than or equal to 1800W and less than or equal to 2000W;
[0040] The power output by the low-frequency RF power supply in the second sub-etching step is greater than or equal to 1400W and less than or equal to 1600W.
[0041] In some embodiments, the power output by the upper DC power supply in the second sub-etching step is greater than the power output by the upper DC power supply in the second plasma etching step.
[0042] In some embodiments, the power output by the upper DC power supply in the second sub-etching step is greater than or equal to 400 W and less than or equal to 500 W.
[0043] In some embodiments, the fourth gas combination includes a carbon-fluorine gas having a ratio of fluorine to carbon greater than or equal to 2 and a third inert gas.
[0044] In some embodiments, the flow rate of the fluorine-to-carbon gas having a ratio of fluorine to carbon greater than or equal to 2 is 8% to 12% of the flow rate of the third inert gas.
[0045] In some embodiments, the flow rate of the third inert gas is greater than or equal to 900 sccm and less than or equal to 1100 sccm;
[0046] The flow rate of the carbon-fluorine gas in which the ratio of the fluorine element to the carbon element is greater than or equal to 2 is greater than or equal to 90 sccm and less than or equal to 110 sccm.
[0047] In some embodiments, the first sub-etching step and the second sub-etching step are cyclically performed at least twice.
[0048] In some embodiments, a ratio of a process duration of the second sub-etching step to a process duration of the first sub-etching step is greater than or equal to 1 and less than or equal to 2.
[0049] In some embodiments, the first plasma etching step, the second plasma etching step, and the third plasma etching step are cyclically performed at least twice.
[0050] The present invention has the following beneficial effects:
[0051] The chamber cleaning method provided by the present invention can adopt a first plasma etching step and a second plasma etching step to first remove the organic polymer on the surface in contact with the plasma in the process chamber, and then remove the inorganic deposits on the surface in contact with the plasma of the designated component in the process chamber and at least one of the organic polymer in the pore structure; it can also adopt the first plasma etching step and the third plasma etching step to sequentially remove the organic polymer and the metal deposition by-product; it can also adopt the first plasma etching step, the second plasma etching step and the third plasma etching step to first remove the organic polymer on the surface in contact with the plasma in the process chamber, and then remove the inorganic deposits on the surface in contact with the plasma of the designated component in the process chamber and at least one of the organic polymer in the pore structure, and finally remove the metal deposition by-product. The above three methods can remove more types of etching by-products, and when the second plasma etching step is adopted, the plasma area in the chamber and other areas away from the plasma area and the organic polymer in the pore structure can be removed, and the area where the organic polymer is removed is more comprehensive.
[0052] Moreover, the present invention removes multiple etching by-products in the above order, and can achieve complete recovery of the chamber environment. Specifically, since organic polymers are usually the encapsulation layer of other etching by-products and are easier to remove, the organic polymers on the surface in contact with the plasma in the process chamber are first removed to reduce the difficulty of removing other by-products in subsequent steps. Then, in the case of a second plasma etching step, inorganic deposits (such as silicon oxide layer) on the surface of the designated components (such as the upper electrode plate, the focusing ring) in the process chamber that are in contact with the plasma are removed, thereby avoiding the reduction of RF feeding efficiency due to excessive accumulation of oxide layer on the upper electrode plate, resulting in process instability; and / or, by removing the organic polymers in the pore structure, a more comprehensive removal of the organic polymers can be achieved. When the third plasma etching step is adopted, metal deposition by-products on the surface in contact with the plasma in the process chamber are removed. Since the accumulation of metal deposition by-products will seriously affect the etching rate, the problem of the etching rate gradually decreasing when the number of processed wafers reaches a certain number or the process time reaches a certain length can be solved by removing the metal deposition by-products, thereby improving the process consistency and repeatability, and further affecting the product yield. BRIEF DESCRIPTION OF THE DRAWINGS
[0053] Figure 1 A graph showing the number of processed wafers and the etching rate in the prior art;
[0054] Figure 2 A flow chart of a chamber cleaning method provided by an embodiment of the present invention;
[0055] Figure 3 A partial cross-sectional view of a CCP device used in an embodiment of the present invention;
[0056] Figure 4 A comparison chart of the cleaning rate and cleaning uniformity of the WLDC process using O2 alone in the prior art and the WLDC process using O2 and CF4 in the present application;
[0057] Figure 5 A partial cross-sectional view of a CCP device used in an embodiment of the present invention with 10 cleaning positions marked thereon;
[0058] Figure 6 The figure is a comparison diagram of the lower surface of the current equalizer plate when the upper DC power supply is not turned on and when the upper DC power supply is turned on.
[0059] Figure 7 A comparison chart of the proportions of Si, C, O and F elements when CEL deposition and Black Si are generated on the lower surface of the flow plate;
[0060] Figure 8 for Figure 7A comparison diagram of the lower surface of the flow plate when CEL deposition is generated and BlackSi is generated;
[0061] Fig. 9 A curve diagram of etching rates corresponding to different numbers of cycles and process durations of the first sub-etching step and the second sub-etching step;
[0062] Fig.10 A curve comparison diagram of the number of wafers and the etching rate in two process steps using the chamber cleaning method provided by the embodiment of the present invention and the prior art;
[0063] Fig.11 The figure is a graph showing the number of processed wafers and the etching rate obtained by using the chamber cleaning method provided by the embodiment of the present invention. DETAILED DESCRIPTION
[0064] In order to enable those skilled in the art to better understand the technical solution of the present invention, the chamber cleaning method provided by the present invention is described in detail below with reference to the accompanying drawings.
[0065] In the prior art, when CCP equipment is used to perform the WLDC process, a plasma formed by O2 with a large flow rate (for example, 800sccm-1500sccm) is used to remove organic polymers. However, although the plasma formed by O2 alone reacts quickly with the polymer, the oxygen free radicals in the plasma have a short residual time in the chamber and cannot fully contact the part of the chamber far away from the plasma area. The polymer in this part cannot be removed and continues to accumulate, eventually causing the etching rate to gradually decrease due to the accumulation of the polymer. Moreover, the upper electrode and the focusing ring in the CCP equipment are made of silicon. The plasma formed by O2 alone will oxidize the silicon parts. For the upper electrode connected to the radio frequency circuit, its oxide layer will affect the radio frequency circuit and cause sparks in severe cases. In addition, the plasma formed by O2 alone does not have the ability to remove metal deposition byproducts, causing metals such as Al, Ti, Ni, Cu, etc. to gradually accumulate in the chamber. Figure 1As shown, the horizontal axis represents the number of processed wafers, and the vertical axis represents the etching rate (ER); Curve 1 represents the voltage peak of the processed wafer (it is a parameter recorded during the wafer run, and the change in this value represents the change in the sheath voltage and plasma, which directly affects the etching rate); Curve 2 represents the voltage peak of the DC (dry clean) process performed after each wafer is processed. The DC process can be specifically a waferless automatic dry etching cleaning (Waferless Auto Dry Clean, referred to as WLDC) process. Analysis of the changing trends of curves 1 and 2 shows that when the number of processed wafers reaches a certain number or the process time reaches a certain length (for example, reaching the moment corresponding to straight line A), the etching rate (ER) will gradually decrease (Start trend down) due to the accumulation of etching by-products, and will drop below the straight line B corresponding to the lowest limit (Low limit, for example, a drop of 2.5%), which not only causes the etching rate to fail to meet the requirements, but also leads to poor process consistency and repeatability, thereby affecting the product yield.
[0066] In order to solve the above problems, an embodiment of the present invention provides a chamber cleaning method, which can eliminate the trend of monotonic change of etching rate (that is, the etching rate gradually decreases) during the mass production process, thereby improving process consistency and repeatability, and further affecting product yield. The method includes a first plasma etching step S1, and also includes at least one of a second plasma etching step S2 and a third plasma etching step S3. That is to say, the method may include the first plasma etching step S1 and the second plasma etching step S2, or may include the first plasma etching step S1 and the third plasma etching step S3, or may include the first plasma etching step S1, the second plasma etching step S2 and the third plasma etching step S3. The above etching steps are performed in sequence. For example, Figure 2 A flow chart is shown for sequentially performing the first plasma etching step S1, the second plasma etching step S2 and the third plasma etching step S3.
[0067] Among them, the first plasma etching step S1 is used to remove organic polymers on the surface in contact with plasma in the process chamber; the second plasma etching step S2 is used to remove inorganic deposits on the surface in contact with plasma of a designated component in the process chamber and at least one of organic polymers in the pore structure; the third plasma etching step S3 is used to remove metal deposition byproducts on the surface in contact with plasma in the process chamber.
[0068] In practical applications, the first plasma etching step S1 and the second plasma etching step S2, or the first plasma etching step S1 and the third plasma etching step S3, or the first plasma etching step S1, the second plasma etching step S2 and the third plasma etching step S3 can be selected according to the types of etching byproducts existing in the process chamber of the semiconductor processing equipment used. For example, if only the organic polymer needs to be removed, the first plasma etching step S1 and the second plasma etching step S2 can be used; for another example, if the organic polymer and metal deposition byproducts need to be removed, the first plasma etching step S1 and the third plasma etching step S3 can be used, or the first plasma etching step S1, the second plasma etching step S2 and the third plasma etching step S3 can be used.
[0069] The chamber cleaning method provided by the embodiment of the present invention can adopt the first plasma etching step and the second plasma etching step to first remove the organic polymer on the surface in contact with the plasma in the process chamber, and then remove the inorganic deposits on the surface in contact with the plasma of the designated component in the process chamber and at least one of the organic polymer in the pore structure; the first plasma etching step and the third plasma etching step can also be adopted to sequentially remove the organic polymer and the metal deposition by-product; the first plasma etching step, the second plasma etching step and the third plasma etching step can also be adopted to first remove the organic polymer on the surface in contact with the plasma in the process chamber, and then remove the inorganic deposits on the surface in contact with the plasma of the designated component in the process chamber and at least one of the organic polymer in the pore structure, and finally remove the metal deposition by-product. The above three methods can remove more types of etching by-products, and when the second plasma etching step is adopted, the organic polymer in the plasma area in the chamber and other areas away from the plasma area and the pore structure can be removed, and the area where the organic polymer is removed is more comprehensive.
[0070] Moreover, the present invention removes multiple etching by-products in the above order, and can achieve complete recovery of the chamber environment. Specifically, since organic polymers are usually the encapsulation layer of other etching by-products and are easier to remove, the organic polymers on the surface in contact with the plasma in the process chamber are first removed to reduce the difficulty of removing other by-products in subsequent steps. Then, in the case of a second plasma etching step, inorganic deposits (such as silicon oxide layer) on the surface of the designated components (such as the upper electrode plate, the focusing ring) in the process chamber that are in contact with the plasma are removed, thereby avoiding the reduction of RF feeding efficiency due to excessive accumulation of oxide layer on the upper electrode plate, resulting in process instability; and / or, by removing the organic polymers in the pore structure, a more comprehensive removal of the organic polymers can be achieved. When the third plasma etching step is adopted, metal deposition by-products on the surface in contact with the plasma in the process chamber are removed. Since the accumulation of metal deposition by-products will seriously affect the etching rate, the problem of the etching rate gradually decreasing when the number of processed wafers reaches a certain number or the process time reaches a certain length can be solved by removing the metal deposition by-products, thereby improving the process consistency and repeatability, and further affecting the product yield.
[0071] The chamber cleaning method provided in the embodiment of the present invention is applied to a capacitively coupled plasma (CCP) device to perform a waferless automatic dry etching cleaning (WLDC) process as an example. Figure 3As shown, the CCP device includes a process chamber 100 and an upper electrode 101 disposed at the top of the process chamber 100 and a lower electrode 102 disposed below the upper electrode 101, wherein the upper electrode 101 is electrically connected to an upper DC power supply, and the upper DC power supply is used to load DC power to the upper electrode 101. The lower electrode 102 is electrically connected to a high-frequency RF power supply and a low-frequency RF power supply (both of which are not shown in the figure), and the high-frequency RF power supply is used to load high-frequency RF power to the lower electrode 102; the low-frequency RF power supply is used to load low-frequency RF power to the lower electrode 102. Specifically, the lower electrode 102, for example, includes an electrostatic chuck (ESC), in which an RF electrode for electrically connecting to the high-frequency RF power supply and the low-frequency RF power supply, and an adsorption electrode for electrically connecting to an adsorption DC power supply are provided. The upper electrode 101, for example, includes a uniform flow plate with multiple air inlets, and the uniform flow plate is made of silicon material as the upper electrode 101 plate at the same time, and is electrically connected to the upper DC power supply (not shown in the figure). When performing the WLDC process, gas is introduced into the process chamber 100 through multiple gas inlets of the flow plate, and the high-frequency RF power supply and / or the low-frequency RF power supply, and / or the upper DC power supply are turned on to excite the gas in the process chamber 100 to form a plasma, and the active particles in the plasma are used to remove the etching byproducts (mainly including inorganic polymers such as silicon-based and silicon-based products, metal deposition byproducts, and organic polymers such as fluorine-containing and carbon-containing products) deposited on the surface of the components exposed to the plasma environment in the process chamber 100. Of course, in practical applications, the chamber cleaning method provided in the embodiment of the present invention can also be applied to other semiconductor processing equipment, such as ICP equipment.
[0072] It should be noted that the upper electrode and the focusing ring in the CCP device are made of silicon. The plasma formed by using O2 alone will oxidize the silicon parts. For the upper electrode connected to the RF circuit, its oxide layer will affect the RF circuit, and in severe cases, it will cause sparks. Based on this, when the chamber cleaning method provided by the embodiment of the present invention is applied to the chamber cleaning of the CCP device, the second plasma etching step S2 can be used to remove the inorganic deposits (such as the oxide layer of silicon) on the surface of the designated parts (such as the upper electrode plate and the focusing ring) in the process chamber of the CCP device that are in contact with the plasma, thereby avoiding the reduction of the RF feeding efficiency due to the excessive accumulation of the oxide layer on the upper electrode plate, resulting in process instability. At the same time, the second plasma etching step S2 can also be used to remove the organic polymer in the pore structure in the process chamber of the CCP device. In practical applications, when the chamber cleaning method provided by the embodiment of the present invention is applied to the chamber cleaning of other semiconductor processing equipment, in the absence of inorganic deposits (such as the oxide layer of silicon), the second plasma etching step S2 is only used to remove the organic polymer in the pore structure in the process chamber. Alternatively, the second plasma etching step S2 can also be omitted.
[0073] The specific implementation methods of the three etching steps for realizing the above functions are described in detail below. Specifically, the above-mentioned first plasma etching step S1 is used to remove organic polymers on the surface in contact with the plasma in the process chamber 100, and the organic polymers include, for example, fluorocarbon polymers. The additional F atoms introduced by the fluorocarbon polymers will cause inconsistent process stability and need to be removed. Moreover, since organic polymers are usually the encapsulation layer of other etching by-products and are easier to remove, the present application first removes the organic polymers on the surface in contact with the plasma in the process chamber 100. When the organic polymer coated on the outer layer is consumed, the high flow rate of O2 can react with the relatively high binding energy complex by-products containing metal components attached to the inner layer to generate by-products with lower binding energy, thereby reducing the difficulty of removing other by-products in subsequent steps.
[0074] In some embodiments, in the first plasma etching step S1, plasma etching is performed using a first gas combination, and the first gas combination includes O2 and CF4.
[0075] Compared with the prior art, the present application does not use O2 alone, but adds CF4 on the basis of O2. By adopting the gas combination of O2 and CF4, CF4 will not only increase the electron density in the plasma, thereby promoting the dissociation of oxygen atoms and generating more active oxygen free radicals, that is, increasing the concentration of oxygen free radicals; moreover, OF free radicals (OF*) can also be generated. OF free radicals can stabilize oxygen free radicals (O*) to prolong the residence time of oxygen free radicals in the chamber so that they can fully react with organic polymers, thereby improving the cleaning ability of organic polymers. At the same time, prolonging the residence time of oxygen free radicals in the chamber can also improve the cleaning ability of organic polymers in the area outside the plasma area of the removal chamber, thereby achieving more comprehensive removal of organic polymers.
[0076] On this basis, carbon-fluorine gases (such as C4F8 and C4F6) with a low ratio of fluorine to carbon are themselves sources of deposited polymers and will introduce polymers. In carbon-fluorine gases containing H, such as CH2F2, hydrogen atoms will combine with fluorine atoms, affecting the generation of F free radicals, which is equivalent to reducing the ratio of fluorine to carbon, and will also introduce polymers. Based on this, the present application uses CF4, which has a higher ratio of fluorine to carbon, to reduce or even avoid the above-mentioned problem of introducing polymers.
[0077] In some embodiments, the flow rate of CF4 is 5‰ to 10‰ of the flow rate of O2. By setting the flow rate of CF4 within this range, the dissociation of oxygen atoms can be effectively promoted. By detecting the spectral signal of O, it is found that compared with using O2 alone, the embodiment of the present invention can increase the content of O in the chamber by about three times by adding CF4 of 5‰ to 10‰ of the flow rate of O2. Moreover, by setting the flow rate of CF4 within this range, the efficiency of removing organic polymers can be maximized. Whether it is higher or lower than this range, the ability to remove organic polymers will be weakened, and CF4 above this range will also have a certain loss effect on the components in the chamber.
[0078] like Figure 4 The figure shows a comparison of the cleaning rate and cleaning uniformity of the WLDC process using O2 alone in the prior art and the WLDC process using O2 and CF4 in the present application. Mean represents the cleaning rate, which is used to reflect the overall cleaning ability. The larger the value, the stronger the cleaning ability. Range represents the difference between the maximum cleaning rate and the minimum cleaning rate in the chamber, which is used to reflect the cleaning uniformity (the uniformity of the cleaning ability at all positions in the chamber). The smaller the value, the better the cleaning uniformity. Figure 4 It can be seen that the Mean value of the WLDC process using O2 and CF4 in the present application is 2.8 times the Mean value of the WLDC process using O2 alone in the prior art, so the WLDC process using O2 and CF4 in the present application can effectively improve the overall cleaning ability. Moreover, the Range value of the WLDC process using O2 and CF4 in the present application is smaller than the Range value of the WLDC process using O2 alone in the prior art, so the WLDC process using O2 and CF4 in the present application can effectively improve the cleaning uniformity.
[0079] Furthermore, in some embodiments, the flow rate of O2 is greater than or equal to 1500 sccm and less than or equal to 2000 sccm; the flow rate of CF4 is greater than or equal to 5 sccm and less than or equal to 20 sccm.
[0080] In some embodiments, the chamber pressure used in the first plasma etching step S1 is greater than the chamber pressure used in the second plasma etching step S2 and the third plasma etching step S3. From the relationship τ=PV / Q, where τ is the residence time of oxygen free radicals in the chamber; P is the chamber pressure; V is the chamber volume; and Q is the gas flow rate, it can be seen that the residence time τ of oxygen free radicals in the chamber is proportional to the chamber pressure P. The higher the chamber pressure P, the longer the residence time τ, and the oxygen free radicals have enough time to diffuse to the area outside the plasma area. Therefore, the first plasma etching step S1 can extend the residence time of oxygen free radicals in the chamber by using a relatively high chamber pressure. It is preferably used in conjunction with the addition of CF4 to more effectively improve the cleaning ability of removing organic polymers in the area outside the plasma area in the chamber, thereby achieving more comprehensive removal of organic polymers. Figure 5 As shown, the areas outside the plasma area in the process chamber 100 include, for example, the upper ceramic ring 103, the chamber wall (or the side wall of the liner 104), the exhaust ring 105, the side wall of the lower electrode 102, etc. These areas are also the locations where organic polymers are most easily deposited.
[0081] Furthermore, in some embodiments, the chamber pressure used in the first plasma etching step S1 to achieve the above effect is greater than or equal to 700 mT and less than or equal to 850 mT.
[0082] In some embodiments, in the first plasma etching step S1, the upper DC power supply is turned off; the low-frequency RF power supply and the high-frequency RF power supply are turned on. It should be noted that the high-frequency RF power supply is used to load high-frequency RF power to the lower electrode 102, and its main function is to increase the electron concentration and generate high-density plasma; the low-frequency RF power supply is used to load low-frequency RF power to the lower electrode 102, and its main function is to generate plasma, and the effect of increasing plasma concentration is weaker than that of high-frequency RF power, but low-frequency RF power can increase plasma energy and enhance bombardment. The upper DC power supply is used to load DC power to the upper electrode 101, which plays an auxiliary role in the process, mainly used to further increase the plasma density, and can also increase the thickness of the sheath of the upper electrode 101 to play a role in cleaning the upper electrode 101. Based on this, the first plasma etching step S1 can generate high-density plasma, increase plasma energy, enhance bombardment, and improve the ability to remove organic polymers by turning on the low-frequency RF power supply and the high-frequency RF power supply. In addition, the first plasma etching step S1 is mainly used to remove organic polymers, and the upper DC power supply can be turned off.
[0083] On this basis, the ratio of the power output of the RF power supply at high frequency to the power output of the RF power supply at low frequency in the first plasma etching step S1 is greater than the ratio of the power output of the RF power supply at high frequency to the power output of the RF power supply at low frequency in the second plasma etching step S2. It should be noted that in CCP equipment, the maximum total power of the RF power supply at high frequency and the RF power supply at low frequency is basically around 4000W. The maximum total power will be limited at the factory end to prevent the chamber from being damaged by excessive power due to misoperation. In order to reserve a certain safety range, in the actual process, the total power is usually set at around 3500W. For example, in order to obtain the most efficient cleaning effect, the total power of the RF power supply at high frequency and the RF power supply at low frequency can be maintained at any value in the range of 3200W to 3600W or change slightly. In this case, if the power output of the RF power supply at high frequency needs to be increased, the power output of the RF power supply at low frequency needs to be reduced accordingly to ensure that the total power remains unchanged or changes slightly; conversely, if the power output of the RF power supply at high frequency needs to be reduced, the power output of the RF power supply at low frequency needs to be increased accordingly to ensure that the total power remains unchanged or changes slightly.
[0084] In the first plasma etching step S1, in order to improve the ratio of the power output of the RF power supply at high frequency to the power output of the RF power supply at low frequency, a relatively high power output of the RF power supply at high frequency is used, and a relatively low power output of the RF power supply at low frequency is used. The relatively high power output of the RF power supply at high frequency can make the combined gas of O2 and CF4 dissociate more active components, that is, increase the dissociation of oxygen molecules to obtain more active oxygen free radicals, so as to further increase the concentration of oxygen free radicals and improve the cleaning ability of organic polymers. On this basis, combined with the use of a relatively low power output of the RF power supply at low frequency, not only can the organic polymer in the gap between the lower electrode 102 and the focusing ring 107 be effectively removed, but also the low power output of the RF power supply at low frequency can prevent the focusing ring 107 and the shielding ring 108 from excessive consumption, causing other problems of subsequent products.
[0085] Furthermore, in some embodiments, in order to better achieve the above effects, the power output of the RF power supply at high frequency in the first plasma etching step S1 is greater than or equal to 1900 W and less than or equal to 2100 W; the power output of the RF power supply at low frequency in the first plasma etching step S1 is greater than or equal to 900 W and less than or equal to 1100 W.
[0086] In some embodiments, the process time of the first plasma etching step S1 is greater than or equal to 85 seconds and less than or equal to 95 seconds.
[0087] Through experiments, it was found that Figure 5As shown, in combination with the following Table 1, position 1 is the center position of the flow plate (i.e., the lower electrode 101); position 2 is the edge position of the flow plate (i.e., the lower electrode 101); position 3 is the inner ring position of the upper ceramic ring 103; position 4 is the outer ring position of the upper ceramic ring 103; position 5 is the position of the focusing ring 107; position 6 is the position of the shielding ring 108; position 7 is the top position of the side wall of the liner 104; position 8 is the bottom position of the side wall of the liner 104; position 9 is the position of the exhaust ring 105; position 10 is the position of the grounding ring 106.
[0088] Table 1
[0089]
[0090] It can be seen from Table 1 that, compared with the cleaning rate of the prior art for the 10 cleaning positions in the chamber, the cleaning rate of the first plasma etching step S1 for the 10 cleaning positions is significantly higher than that of the prior art, and the cleaning rate multiple is about 4 to 13 times, especially at positions 3, 4, 7, 8 and 9, which are all parts with large exposed surfaces. The present application greatly improves the cleaning ability of these parts.
[0091] The second plasma etching step S2 is used to remove at least one of inorganic deposits (such as inorganic oxides) on the surface of the designated component in the process chamber 100 in contact with the plasma and organic polymers in the pore structure. Taking the chamber cleaning method provided in the embodiment of the present invention as an example of chamber cleaning of CCP equipment, the designated component includes but is not limited to the upper electrode 101 (such as a flow plate), the lower surface of the upper electrode 101 is in contact with the plasma, and inorganic deposits such as silicon-based and silicon-based products are easily deposited. Taking the upper electrode 101 as an example of silicon material, the inorganic deposits deposited on the surface of the upper electrode 101 in contact with the plasma are silicon oxide. Too much oxide layer accumulated in the upper electrode 101 will cause the RF feeding efficiency to decrease, resulting in process instability. The above-mentioned pore structure includes but is not limited to the gap structure between the electrostatic chuck (i.e., the lower electrode 102) and the focusing ring 107, and the gap structure between the focusing ring 107 and the shielding ring 108. The temperature in these gap structures is relatively low, and organic polymers are easily deposited, and it is not easy for plasma to reach these gap structures, resulting in greater cleaning difficulty.
[0092] In order to achieve the removal of inorganic deposits on the surface of the designated component in the process chamber 100 that is in contact with the plasma and the organic polymer in the pore structure, in some embodiments, in the second plasma etching step S2, the upper DC power supply, the low-frequency RF power supply and the high-frequency RF power supply are turned on. By turning on the low-frequency RF power supply and the high-frequency RF power supply, high-density plasma can be generated, and the plasma energy can be increased, and the bombardment effect can be enhanced to improve the removal ability of organic polymers in the pore structure. On this basis, by turning on the upper DC power supply, the sheath thickness of the upper electrode 101 can be increased to play a role in cleaning the upper electrode 101, thereby improving the ability to remove inorganic deposits on the surface of the upper electrode 101 (such as a uniform flow plate) that is in contact with the plasma. For example, Figure 6 As shown, when the upper DC power supply is not turned on (ie, DC = 0V), the lower surface (ie Figure 3 When the upper DC power supply (eg, DC=300V) is turned on, the lower surface of the flow plate is smooth and has no deposits.
[0093] In some embodiments, the ratio of the power output of the RF power supply at high frequency to the power output of the RF power supply at low frequency in the second plasma etching step S2 is smaller than that in the second plasma etching step S2. Under the condition of the same total power, the power output of the RF power supply at high frequency in the second plasma etching step S2 is relatively low, and at the same time, the power output of the RF power supply at low frequency in the second plasma etching step S2 is relatively high, which can more effectively improve the removal ability of organic polymers in the pore structure.
[0094] Furthermore, in some embodiments, in order to better achieve the above-mentioned effects, the power output of the RF power supply at high frequency in the second plasma etching step S2 is greater than or equal to 1300 W and less than or equal to 1500 W; the power output of the RF power supply at low frequency in the second plasma etching step S2 is greater than or equal to 1500 W and less than or equal to 1700 W.
[0095] In some embodiments, in order to better improve the ability to remove inorganic deposits on the surface of the upper electrode 101 (such as a flow plate) in contact with the plasma, the power output by the upper DC power supply in the second plasma etching step S2 is greater than or equal to 300W and less than or equal to 400W.
[0096] In some embodiments, the chamber pressure used in the second plasma etching step S2 is less than the chamber pressure used in the first plasma etching step S1. The chamber pressure used in the second plasma etching step S2 can be switched from a higher value to a lower value when switching from the first plasma etching step S1 to the second plasma etching step S2 by using a relatively low chamber pressure. Under the condition that the intake flow rate of the first plasma etching step S1 and the second plasma etching step S2 is basically the same, the reduction of the chamber pressure is the increase of the exhaust flow rate of the process chamber (for example, the opening of the exhaust flow regulating valve is increased), which improves the gas flowability in the process chamber and generates disturbances in the air flow to generate gas field vibration in the chamber. The gas field vibration can play a role in flushing the intake channel of the upper electrode 101 (for example, the uniform flow plate) and the organic polymer in the pore structure. On the other hand, the mean free path can also be increased, so that the plasma can enter the gap structure of the lower electrode 102, bombard the organic polymer in the gap structure, and the bombarded polymer can be discharged from the chamber with the air flow.
[0097] In some embodiments, in order to achieve the above effects, the chamber pressure used in the second plasma etching step S2 is greater than or equal to 45 mT and less than or equal to 60 mT.
[0098] In some embodiments, in the second plasma etching step S2, plasma etching is performed using a second gas combination; the second gas combination includes O2, a carbon fluorine gas, and a first inert gas.
[0099] In some embodiments, the carbon-fluorine gas that realizes the above functions includes, for example, at least one of C4F8 and C4F6.
[0100] The plasma formed by the first inert gas is used to enhance the bombardment capability of the organic polymer entering the gap structure of the lower electrode 102. The addition of the first inert gas in conjunction with the use of a lower chamber pressure can enhance the bombardment capability. In addition, the first inert gas is also used as a carrier gas to carry the bombarded polymer out of the chamber. In a preferred embodiment, the first inert gas includes Ar. On the one hand, Ar is larger than the atoms of He and Ne and has a stronger bombardment capability. On the other hand, Ar is cheaper than some inert gases (such as Kr).
[0101] In some embodiments, in order to better achieve the above effect, the flow rate of the first inert gas is greater than or equal to 1000 sccm and less than or equal to 1200 sccm.
[0102] O2 is used to remove organic polymers in the pore structure. The plasma formed by the fluorocarbon gas is used to remove inorganic deposits on the surface of the upper electrode 101 (such as the flow plate) in contact with the plasma. On this basis, the combination of O2 and the fluorocarbon gas can achieve a balance between the ability to remove inorganic deposits on the upper electrode 101 (such as the flow plate) and prevent the upper electrode 101 from being oxidized. Specifically, the balance can be achieved by controlling the flow ratio of the two.
[0103] like Figure 7 As shown, if the second plasma etching step S2 does not use O2, that is, O2=0, a polymer will be deposited on the upper electrode 101 due to the excessive flow of the fluorocarbon gas. At this time, the surface composition of the upper electrode 101 includes a fluorocarbon polymer (CFx). The actual surface of the upper electrode 101 is as shown in FIG. Figure 8 As shown in the left figure, there is a polymer on its surface. If the second plasma etching step S2 uses an O2 flow rate that is too large, for example, O2 = 50 sccm, the surface of the upper electrode 101 is oxidized. At this time, the surface components of the upper electrode 101 (for example, silicon) include silicon oxide (SiO). Since F radicals etch Si faster and etch silicon oxide slower, the surface of the upper electrode 101 is bumpy, that is, the following is produced: Figure 8 The actual surface shown in the right picture is black silicon (Black Si).
[0104] In order to solve the above problem, in some embodiments, the ratio of the flow rate of the fluorocarbon gas to the flow rate of O2 is greater than or equal to 2 and less than or equal to 3. By making the above ratio satisfy this numerical range, it is possible to avoid the formation of fluorocarbon polymers on the surface of the upper electrode 101 due to excessive flow rate of the fluorocarbon gas, and to avoid the oxidation of the upper electrode 101 due to excessive flow rate of O2, thereby generating black silicon (Black Si) and causing subsequent mass production problems.
[0105] On this basis, the combination of O2 and fluorocarbon gas, in conjunction with turning on the upper DC power supply, can both enhance the cleaning effect on the upper electrode 101 to prevent the addition of fluorocarbon gas from depositing fluorocarbon polymers on the upper electrode 101, and prevent the addition of O2 from forming oxidized deposits on the upper electrode 101, thereby protecting the upper electrode 101 and avoiding the generation of black silicon problems.
[0106] Furthermore, in some embodiments, in order to better achieve the above effects, the flow rate of O2 is greater than or equal to 20 sccm and less than or equal to 30 sccm; the flow rate of the fluorocarbon gas is greater than or equal to 40 sccm and less than or equal to 60 sccm. Figure 7As shown, if the second plasma etching step S2 adopts an O2 flow rate of 20 sccm, a balance can be achieved between the ability to remove inorganic deposits on the upper electrode 101 (such as a uniform flow plate) and preventing the upper electrode 101 from being oxidized. This can prevent the carbon fluorine gas flow rate from being too large to cause carbon fluorine polymers to form on the surface of the upper electrode 101, and can also prevent the O2 flow rate from being too large to cause oxidation of the upper electrode 101, thereby generating black silicon (Black Si) and causing subsequent mass production problems.
[0107] In some embodiments, the process time of the second plasma etching step S2 is greater than or equal to 55 s and less than or equal to 65 s.
[0108] The third plasma etching step S3 is used to remove metal deposition byproducts on the surface in contact with the plasma in the process chamber 100. Since the accumulation of metal deposition byproducts will seriously affect the etching rate, the problem of the etching rate gradually decreasing when the number of processed wafers reaches a certain number or the process time reaches a certain length of time can be solved by removing the metal deposition byproducts, thereby improving the process consistency and repeatability, thereby affecting the product yield.
[0109] In some embodiments, in order to remove the metal deposition byproducts on the surface in contact with the plasma in the process chamber 100, the third plasma etching step S3 includes:
[0110] In a first sub-etching step, a plasma formed by a third gas combination is used to perform a reduction reaction on the metal deposition byproducts;
[0111] In the second sub-etching step, the plasma formed by the fourth gas combination is used to physically bombard the products generated by the reduction reaction, so that the bombarded products are discharged from the chamber along with the gas flow.
[0112] The third plasma etching step S3 can firstly perform a reduction reaction on the metal deposition byproducts to generate products with lower binding energy by using two sub-etching steps; then physically bombard the products with lower binding energy generated by the reduction reaction so that the bombarded products can be discharged from the chamber with the airflow, that is, two sub-etching steps are used to jointly achieve the removal of the metal deposition byproducts. Experiments have shown that the use of two sub-etching steps can effectively improve the removal capacity of metal deposition byproducts, for example, 5 times the removal capacity of using Ar alone, and 30 times the removal capacity of using N2 and H2. In addition, the third plasma etching step S3 also has a certain ability to remove inorganic deposits on the surface of the upper electrode 101 (such as a uniform flow plate) that contacts the plasma. In this case, the second plasma etching step S2 can be omitted according to specific circumstances.
[0113] In some embodiments, since the metal deposition byproducts are difficult to remove, the first sub-etching step and the second sub-etching step can be cyclically performed at least twice. In this way, the metal deposition byproducts can be gradually stripped off, and the metal deposition byproducts can be completely removed in the end. Furthermore, in some embodiments, the number of cycles is, for example, greater than or equal to 8, and less than or equal to 15. By adopting this numerical range, the metal deposition byproducts can be effectively removed, the chamber environment can be reset, and the loss of chamber components can be reduced. Preferably, the number of cycles is equal to 8, the ability to remove metal deposition byproducts is the best, and it is the minimum number of cycles that can reduce the loss of chamber components.
[0114] In some embodiments, the third gas combination includes H2 and a second inert gas. The plasma generated by H2 can react with the metal deposition byproducts to generate compounds with lower binding energy. In other words, the effect of the first sub-etching step is similar to surface treatment, and the metal deposition byproducts are not actually removed. The second inert gas is used as a protective gas to prevent H2 ignition explosion and to protect the cleaned upper electrode 101 from being re-oxidized. The second inert gas is also used as a carrier gas for hydrogen and as a cleaning gas to remove polymers that may be produced in the second sub-etching step.
[0115] In some embodiments, in order to better achieve the above effect, the ratio of the flow rate of the second inert gas to the flow rate of H2 is greater than or equal to 4 and less than or equal to 7.
[0116] Furthermore, in some embodiments, the flow rate of the second inert gas is greater than or equal to 250 sccm and less than or equal to 350 sccm; the flow rate of H2 is greater than or equal to 40 sccm and less than or equal to 60 sccm.
[0117] In some preferred embodiments, the second inert gas includes, for example, N2. However, the embodiments of the present invention are not limited thereto, and in practical applications, the second inert gas may also be other inert gases, such as Ar, etc. However, the cleaning effect of the combination of H2 and Ar is relatively weaker than that of the combination of N2 and Ar.
[0118] In some embodiments, the chamber pressure used in the first sub-etching step is less than the chamber pressure used in the first plasma etching step S1. The chamber pressure used in the first sub-etching step can increase the mean free path by using a relatively low chamber pressure, thereby improving the weak bombardment activation effect on the metal byproducts, so that the products with lower binding energy generated by the reduction reaction can be more easily bombarded out in the second sub-etching step.
[0119] In some embodiments, in order to achieve the above effects, the chamber pressure used in the first sub-etching step is greater than or equal to 45 mT and less than or equal to 60 mT.
[0120] In some embodiments, in the first sub-etching step, the high-frequency RF power supply is turned on, and the upper DC power supply and the low-frequency RF power supply are not turned on. Since H atoms are small and easily dissociated, only the high-frequency RF power supply needs to be turned on, and the power output by the high-frequency RF power supply in the first sub-etching step is less than the power output by the high-frequency RF power supply in the second sub-etching step, that is, the first sub-etching step uses a relatively low power output by the high-frequency RF power supply, and sufficient active hydrogen radicals can be obtained to perform a reduction reaction with the metal deposition by-products. In addition, the above-mentioned first sub-etching step is mainly used for the reduction reaction with the metal deposition by-products, and the upper DC power supply can be selected not to be turned on.
[0121] Furthermore, in some embodiments, in order to achieve the above effect, the power output by the RF power supply at high frequency in the first sub-etching step is greater than or equal to 700 W and less than or equal to 800 W.
[0122] The second sub-etching step is a step that actually removes the metal deposition byproducts, that is, physically bombarding the products generated by the reduction reaction in the first sub-etching step so that the bombarded products are discharged from the chamber with the airflow. In some embodiments, in order to physically bombard the products generated by the reduction reaction so that the bombarded products are discharged from the chamber with the airflow, in the second sub-etching step, the upper DC power supply, the low-frequency RF power supply and the high-frequency RF power supply are turned on. By turning on the low-frequency RF power supply and the high-frequency RF power supply, high-density plasma can be generated, plasma energy can be increased, and the bombardment effect can be enhanced. Moreover, the bombardment effect is mainly contributed by the RF power loaded by the low-frequency RF power supply and the high-frequency RF power supply to the lower electrode 102. On this basis, by turning on the upper DC power supply, the bombardment on the top of the chamber can be enhanced, thereby improving the removal ability of the metal deposition byproducts on the top of the chamber.
[0123] Further, in some embodiments, the sum of the power output by the high frequency RF power supply and the power output by the low frequency RF power supply in the second sub-etching step is greater than the sum of the power output by the high frequency RF power supply and the power output by the low frequency RF power supply in the first plasma etching step S1. That is, the total power of the high frequency RF power supply and the low frequency RF power supply in the second sub-etching step is relatively high, so that both the high frequency RF power supply and the low frequency RF power supply can use relatively high power, thereby obtaining a more efficient cleaning effect and ensuring that the metal deposition byproducts can be completely removed.
[0124] In some embodiments, in order to achieve the above effects, the power output of the RF power supply at high frequency in the second sub-etching step is greater than or equal to 1800W and less than or equal to 2000W; the power output of the RF power supply at low frequency in the second sub-etching step is greater than or equal to 1400W and less than or equal to 1600W.
[0125] In some embodiments, in order to achieve the above effect, the power output by the upper DC power supply in the second sub-etching step is greater than the power output by the upper DC power supply in the second plasma etching step S2. By using a relatively high power, the upper DC power supply in the second sub-etching step can further enhance the bombardment of the chamber top, thereby improving the removal capability of the metal deposition byproducts on the chamber top.
[0126] In some embodiments, in order to achieve the above effect, the power output by the upper DC power supply in the second sub-etching step is greater than or equal to 400 W and less than or equal to 500 W.
[0127] In some embodiments, the chamber pressure used in the second sub-etching step is lower than the chamber pressure used in the first plasma etching step S1. The chamber pressure used in the second sub-etching step can increase the mean free path by using a relatively low chamber pressure, thereby enhancing the bombardment capability so as to bombard out the products with lower binding energy generated by the reduction reaction.
[0128] In some embodiments, in order to achieve the above effect, the chamber pressure used in the second sub-etching step is greater than or equal to 45 mT and less than or equal to 60 mT.
[0129] In some embodiments, in the second sub-etching step, the fourth gas combination includes a carbon-fluorine gas with a ratio of fluorine to carbon greater than or equal to 2 and a third inert gas. The carbon-fluorine gas with a ratio of fluorine to carbon greater than or equal to 2 includes, for example, CF4; the plasma generated by the third inert gas is used to bombard the metal deposition byproducts, and the third inert gas is preferably Ar, which has larger atoms and can enhance the bombardment effect. On this basis, by adding CF4, a large number of F radicals can be introduced, and this gas combination can perform physical and chemical etching, that is, bombardment activation and chemical etching are combined, thereby effectively improving the ability to remove metal deposition byproducts.
[0130] In some embodiments, in the second sub-etching step, the flow rate of the fluorine-carbon gas having a ratio of fluorine to carbon greater than or equal to 2 is 8% to 12% of the flow rate of the third inert gas. It is found through experiments that adding 8% to 12% of the flow rate of the fluorine-carbon gas having a ratio of fluorine to carbon greater than or equal to 2 can increase the removal capacity of metal deposition byproducts to 3.4 times the removal capacity of the third inert gas alone.
[0131] In some embodiments, in order to achieve the above effects, the flow rate of the third inert gas is greater than or equal to 900 sccm and less than or equal to 1100 sccm; the flow rate of CF4 is greater than or equal to 90 sccm and less than or equal to 110 sccm.
[0132] In some embodiments, the ratio of the process duration of the second sub-etching step to the process duration of the first sub-etching step is greater than or equal to 1, and less than or equal to 2. By adopting this numerical range, it is possible to effectively remove metal deposition byproducts, achieve the reset of the chamber environment, and reduce the loss of chamber components. Preferably, the ratio of the process duration of the second sub-etching step to the process duration of the first sub-etching step is equal to 1, which has the best ability to remove metal deposition byproducts and is the minimum process duration that can reduce the loss of chamber components. In addition, in actual applications, this ratio can be considered in combination with the above-mentioned number of cycles to obtain better results. For example, if Fig. 9 As shown, the ordinate represents the ability to remove metal deposition byproducts. When the ratio of the process time of the second sub-etching step to the process time of the first sub-etching step is equal to 1, the process time is 7s, and the number of cycles is equal to 8, the ability to remove metal deposition byproducts is the best.
[0133] In some embodiments, the process duration of the second sub-etching step and the process duration of the first sub-etching step are both greater than or equal to 5 s and less than or equal to 10 s, for example.
[0134] In some embodiments, during the first sub-etching step and the second sub-etching step, the chamber temperature is maintained at a high temperature, such as 150° C., which can improve the reaction activation and volatilization effect of metal deposition byproducts.
[0135] In some embodiments, the first plasma etching step S1, the second plasma etching step S2, and the third plasma etching step S3 are cyclically performed at least twice. By cyclically performing the three plasma etching steps, it can be ensured that the chamber is completely reset, that is, the various etching byproducts in the chamber are substantially removed. The number of cycles is, for example, 3 to 5 times.
[0136] like Fig.10As shown, the left and right figures are comparison diagrams of curves 1 and 2 of BARC step (Bottom anti-reflection coating, BARC etching step) and ASH step (ashing step), respectively. Among them, BARC step and ASH step are two process steps in the mass production process recipe. Curve 1 is a curve of the number of wafers and etching rate in the prior art; curve 2 is a curve of the number of wafers and etching rate obtained by the method of the present invention; among them, the prior art is to perform a WLDC process after each wafer is processed, and the present application is based on performing a WLDC process after each wafer is processed. When the number of processed wafers reaches a certain number or the process time reaches a certain length, the chamber cleaning method provided by the embodiment of the present invention is used to reset the environment of the process chamber. By comparing curves 1 and 2, it can be seen that the etching rate (ER) of curve 1 will gradually decrease due to the accumulation of etching by-products, which not only causes the etching rate to fail to meet the requirements, but also leads to poor process consistency and repeatability, thereby affecting the product yield. The etching rate (ER) of curve 2 is smoother than that of curve 1, which can improve process consistency and repeatability, thereby affecting product yield.
[0137] like Fig.11 As shown, the horizontal axis represents the number of processed wafers, and the vertical axis represents the etching rate (ER); Curve 1 represents the voltage peak of the processed wafer (it is a parameter recorded when the wafer is running, and the change in this value represents the change in the sheath voltage and plasma, which directly affects the etching rate); Curve 2 represents the voltage peak of the DC (dry clean) process performed after the processing of each wafer is completed. The DC process can specifically be a waferless automatic dry etching cleaning (Waferless AutoDry Clean, referred to as WLDC) process. Curve 3 represents the voltage peak of the first wafer in each wafer box (Production slot 1). When the number of processed wafers reaches a certain number or the process time reaches a certain length of time (for example, reaching the moment corresponding to straight line D), the chamber cleaning method (i.e., I-DCS) provided in an embodiment of the present invention is used to clean the process chamber 100 to achieve chamber cleaning, by Fig.11 It can be seen that after using the chamber cleaning method provided by the embodiment of the present invention, in the process of continuing to process the wafer (i.e., the process after the moment corresponding to the straight line D), the etching rate (ER) of curves 1-3 is different from that of the prior art (such as Figure 1 Compared with the above, there is no gradual decline, and the etching rate basically meets the requirements, thereby improving the process consistency and poor repeatability, and further improving the product yield.
[0138] In summary, the chamber cleaning method provided by the embodiment of the present invention can adopt the first plasma etching step and the second plasma etching step to first remove the organic polymer on the surface in contact with the plasma in the process chamber, and then remove the inorganic deposits on the surface in contact with the plasma of the designated component in the process chamber and at least one of the organic polymers in the pore structure; the first plasma etching step and the third plasma etching step can also be adopted to sequentially remove the organic polymer and the metal deposition by-product; the first plasma etching step, the second plasma etching step and the third plasma etching step can also be adopted to first remove the organic polymer on the surface in contact with the plasma in the process chamber, and then remove the inorganic deposits on the surface in contact with the plasma of the designated component in the process chamber and at least one of the organic polymers in the pore structure, and finally remove the metal deposition by-product. The above three methods can remove more types of etching by-products, and when the second plasma etching step is adopted, the organic polymer in the plasma area in the chamber and other areas away from the plasma area and the pore structure can be removed, and the area where the organic polymer is removed is more comprehensive.
[0139] Moreover, the present invention removes multiple etching by-products in the above order, and can achieve complete recovery of the chamber environment. Specifically, since organic polymers are usually the encapsulation layer of other etching by-products and are easier to remove, the organic polymers on the surface in contact with the plasma in the process chamber are first removed to reduce the difficulty of removing other by-products in subsequent steps. Then, in the case of a second plasma etching step, inorganic deposits (such as silicon oxide layer) on the surface of the designated components (such as the upper electrode plate, the focusing ring) in the process chamber that are in contact with the plasma are removed, thereby avoiding the reduction of RF feeding efficiency due to excessive accumulation of oxide layer on the upper electrode plate, resulting in process instability; and / or, by removing the organic polymers in the pore structure, a more comprehensive removal of the organic polymers can be achieved. When the third plasma etching step is adopted, metal deposition by-products on the surface in contact with the plasma in the process chamber are removed. Since the accumulation of metal deposition by-products will seriously affect the etching rate, the problem of the etching rate gradually decreasing when the number of processed wafers reaches a certain number or the process time reaches a certain length can be solved by removing the metal deposition by-products, thereby improving the process consistency and repeatability, and further affecting the product yield.
[0140] It is to be understood that the above embodiments are merely exemplary embodiments used to illustrate the principles of the present invention, but the present invention is not limited thereto. For those of ordinary skill in the art, various modifications and improvements can be made without departing from the spirit and essence of the present invention, and these modifications and improvements are also considered to be within the scope of protection of the present invention.
Claims
1. A chamber cleaning method, characterized in that: include: The first plasma etching step further includes at least one of a second plasma etching step and a third plasma etching step; The first plasma etching step is used to remove organic polymers on the surface in contact with the plasma in the process chamber; The second plasma etching step is used to remove at least one of inorganic deposits on the surface of the designated component in the process chamber that contacts the plasma and organic polymers in the pore structure; The third plasma etching step is used to remove metal deposition byproducts on the surface in contact with the plasma in the process chamber.
2. The chamber cleaning method according to claim 1, characterized in that: In the first plasma etching step, plasma etching is performed using a first gas combination; The first gas combination includes O2 and CF4.
3. The chamber cleaning method according to claim 2, characterized in that: The flow rate of CF4 is 5‰ to 10‰ of the flow rate of O2.
4. The chamber cleaning method according to claim 3, characterized in that: The flow rate of O2 is greater than or equal to 1500 sccm and less than or equal to 2000 sccm; The flow rate of CF4 is greater than or equal to 5 sccm and less than or equal to 20 sccm.
5. The chamber cleaning method according to claim 1, characterized in that: The chamber pressure used in the first plasma etching step is greater than that in the second plasma etching step.
6. The chamber cleaning method according to claim 5, characterized in that: The chamber pressure used in the second plasma etching step is greater than or equal to 45 mT and less than or equal to 60 mT.
7. The chamber cleaning method according to claim 1, characterized in that: In the second plasma etching step, turning on the upper DC power supply, the low-frequency lower RF power supply and the high-frequency lower RF power supply; The power output by the upper DC power supply in the second plasma etching step is greater than or equal to 300 W and less than or equal to 400 W; The power outputted by the radio frequency power supply at high frequency in the second plasma etching step is greater than or equal to 1300 W and less than or equal to 1500 W; The power output by the low-frequency RF power supply in the second plasma etching step is greater than or equal to 1500W and less than or equal to 1700W.
8. The chamber cleaning method according to claim 1, characterized in that: In the second plasma etching step, plasma etching is performed using a second gas combination; The second gas combination includes O2, a carbon-fluorine gas and a first inert gas.
9. The chamber cleaning method according to claim 8, characterized in that: The carbon-fluorine gas includes at least one of C4F8 and C4F6.
10. The chamber cleaning method according to claim 8, characterized in that: The ratio of the flow rate of the fluorocarbon gas to the flow rate of O2 is greater than or equal to 2 and less than or equal to 3.
11. The chamber cleaning method according to claim 10, characterized in that: The flow rate of O2 is greater than or equal to 20 sccm and less than or equal to 30 sccm; The flow rate of the fluorocarbon gas is greater than or equal to 40 sccm and less than or equal to 60 sccm.
12. The chamber cleaning method according to claim 1, characterized in that: The third plasma etching step comprises: In a first sub-etching step, a plasma formed by a third gas combination is used to perform a reduction reaction on the metal deposition byproduct; In the second sub-etching step, the plasma formed by the fourth gas combination is used to physically bombard the products generated by the reduction reaction, so that the bombarded products are discharged from the chamber along with the gas flow.
13. The chamber cleaning method according to claim 12, characterized in that: The third gas combination includes H 2 and a second inert gas.
14. The chamber cleaning method according to claim 13, characterized in that: The ratio of the flow rate of the second inert gas to the flow rate of H2 is greater than or equal to 4 and less than or equal to 7.
15. The chamber cleaning method according to claim 14, characterized in that: The flow rate of the second inert gas is greater than or equal to 250 sccm and less than or equal to 350 sccm; The flow rate of H2 is greater than or equal to 40 sccm and less than or equal to 60 sccm.
16. The chamber cleaning method according to claim 12, characterized in that: In the first sub-etching step, the high frequency lower RF power supply is turned on, and the upper DC power supply and the low frequency lower RF power supply are turned off; The power output by the RF power supply at the high frequency in the first sub-etching step is less than the power output by the RF power supply at the high frequency in the second sub-etching step.
17. The chamber cleaning method according to claim 16, characterized in that: The power output by the radio frequency power supply at high frequency in the first sub-etching step is greater than or equal to 700W and less than or equal to 800W.
18. The chamber cleaning method according to claim 12, characterized in that: In the second sub-etching step, turning on the upper DC power supply, the lower low-frequency RF power supply and the lower high-frequency RF power supply; The sum of the power output by the RF power supply at high frequency and the power output by the RF power supply at low frequency in the second sub-etching step is greater than the sum of the power output by the RF power supply at high frequency and the power output by the RF power supply at low frequency in the first plasma etching step.
19. The chamber cleaning method according to claim 18, characterized in that: The power outputted by the radio frequency power supply at high frequency in the second sub-etching step is greater than or equal to 1800W and less than or equal to 2000W; The power output by the low-frequency RF power supply in the second sub-etching step is greater than or equal to 1400W and less than or equal to 1600W.
20. The chamber cleaning method according to claim 18, characterized in that: The power output by the upper DC power supply in the second sub-etching step is greater than the power output by the upper DC power supply in the second plasma etching step.
21. The chamber cleaning method according to claim 20, characterized in that: The power output by the upper DC power supply in the second sub-etching step is greater than or equal to 400W and less than or equal to 500W.
22. The chamber cleaning method according to claim 12, characterized in that: The fourth gas combination includes a carbon-fluorine gas in which the ratio of fluorine element to carbon element is greater than or equal to 2 and a third inert gas.
23. The chamber cleaning method according to claim 22, characterized in that: The flow rate of the fluorine-to-carbon gas having a ratio of fluorine to carbon greater than or equal to 2 is 8% to 12% of the flow rate of the third inert gas.
24. The chamber cleaning method according to claim 23, characterized in that: The flow rate of the third inert gas is greater than or equal to 900 sccm and less than or equal to 1100 sccm; The flow rate of the carbon-fluorine gas in which the ratio of the fluorine element to the carbon element is greater than or equal to 2 is greater than or equal to 90 sccm and less than or equal to 110 sccm.
25. The chamber cleaning method according to claim 12, characterized in that: The first sub-etching step and the second sub-etching step are cyclically performed at least twice.
26. The chamber cleaning method according to claim 25, characterized in that: The ratio of the process duration of the second sub-etching step to the process duration of the first sub-etching step is greater than or equal to 1 and less than or equal to 2.
27. The chamber cleaning method according to claim 1, characterized in that: The first plasma etching step, the second plasma etching step and the third plasma etching step are cyclically performed at least twice.
Citation Information
Cited By
Cleaning method of cavity and process device in cavity
CN119710627A
Valve and semiconductor processing equipment
CN121452357A