Oxide thin film transistor and manufacturing method thereof

Through atomic layer deposition and ion implantation technology, the thermal stability and deposition quality problems in the top gate self-aligning structure are solved, and the preparation of high-quality oxide films is realized, which is suitable for applications such as DRAM.

CN119008414APending Publication Date: 2024-11-22SHANGHAI JIAOTONG UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410961882.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing metal oxide thin film transistors have thermal stability problems in the top gate self-alignment structure. The heavily doped regions caused by hydrogen diffusion and plasma treatment fail at high temperatures, and the magnetron sputtering deposition method has uneven compositions. Poor repeatability and difficult to accurately regulate film thickness.

Method used

An oxide film is formed by atomic layer deposition, and an N-type heavily doped regions are formed through ion implantation. Combined with annealing treatment, the stability of oxygen vacancies is ensured, and the film is achieved by regulating the proportion of elements.

Benefits of technology

It improves the thermal stability and electrical properties of the oxide film, reduces parasitic capacitance, and realizes high-quality oxide film deposition, which is suitable for applications such as dynamic random access memory (DRAM).

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008414A_ABST
    Figure CN119008414A_ABST
Patent Text Reader

Abstract

The invention provides an oxide thin film transistor and a manufacturing method thereof, and the method comprises the steps: providing a substrate with a buffer layer, and forming an oxide thin film on the buffer layer through an atomic layer deposition mode; carrying out photoetching and wet etching on the oxide thin film to obtain a patterned oxide thin film; annealing the patterned oxide thin film; depositing a gate insulating layer on the annealed patterned oxide thin film; depositing a gate electrode on the gate insulating layer, and performing graphical processing on the gate electrode; performing ion implantation on two ends of the oxide thin film by taking the patterned gate electrode as a mask to form an N-type heavily doped region; etching the gate insulating layer on the N-type heavily doped region by taking the patterned gate electrode as a mask; and depositing metal on the N-type heavily doped region to form a source electrode and a drain electrode, and annealing to obtain the oxide thin film transistor. The components of the oxide thin film can be accurately regulated and controlled, the film forming quality is high, the thin film uniformity is good, and meanwhile the good thermal stability is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of semiconductor devices, and in particular to an oxide thin film transistor and a method for manufacturing the same. Background Art

[0002] In recent years, metal oxide thin film transistors are receiving more and more attention, among which the bottom gate structure is the most commonly used metal oxide thin film transistor structure. However, in the bottom gate structure, there is an overlapping area between the gate and the source and drain, which will produce a large parasitic capacitance. In order to reduce the parasitic capacitance, a top gate self-aligned structure is proposed. In the top gate self-aligned structure, since there is no overlapping area between the gate and the source and drain, the parasitic capacitance is greatly reduced. In order to enhance the gate control capability, the source and drain regions need to be treated as heavily doped regions. The commonly used methods are hydrogen diffusion and plasma treatment, but both methods have thermal stability problems. Hydrogen is an element that is very easy to diffuse. In the top gate self-aligned thin film transistor treated with hydrogen diffusion, hydrogen will diffuse from the source and drain regions to the middle channel region that has not been treated when heated, resulting in a decrease in channel resistance and the device losing its switching characteristics. The principle of plasma treatment to produce heavily doped regions is to generate oxygen vacancies through plasma bombardment. However, after being heated, the oxygen vacancies will recombine with oxygen, causing the source and drain regions to return to high resistance regions and device performance degradation. In fact, thermal stability has always been a major problem facing top-gate self-aligned metal oxide thin film transistors. In addition, the deposition method commonly used for the channel material in transistors, that is, oxide thin films, is magnetron sputtering. Magnetron sputtering has problems such as uneven composition of film deposition, poor repeatability, and difficulty in accurately controlling the film thickness. How to deposit high-quality oxide films so that the devices can be used in dynamic random access memory (DRAM) and the like is also a technical problem that needs to be solved in this field.

[0003] After searching, it was found that the Chinese invention patent with application publication number CN107623040A discloses an indium gallium zinc oxide thin film transistor and its manufacturing method. The patent uses DC direct current magnetron sputtering method or RF radio frequency magnetron sputtering method to deposit indium gallium zinc oxide thin film on buffer layer, uses ion implanter or ion sprayer to implant arsenic ions or phosphorus ions into indium gallium zinc oxide thin film, and then anneals to form N-type heavily doped source and drain regions in indium gallium zinc oxide thin film. The transistor in the prior art serves display application, and still uses sputtering deposition to form oxide thin film, which does not solve the above problems. Summary of the invention

[0004] In view of the defects in the prior art, an object of the present invention is to provide an oxide thin film transistor and a method for manufacturing the same.

[0005] According to one aspect of the present invention, a method for manufacturing an oxide thin film transistor is provided, the method comprising:

[0006] Providing a substrate having a buffer layer, and forming an oxide thin film on the buffer layer by atomic layer deposition;

[0007] sequentially performing photolithography and wet etching on the oxide film to obtain a patterned oxide film;

[0008] annealing the patterned oxide film;

[0009] depositing a gate insulating layer on the annealed patterned oxide film;

[0010] Depositing a gate electrode on the gate insulating layer, and performing a patterning process on the gate electrode;

[0011] Using the patterned gate electrode as a mask, ion implantation is performed on both ends of the oxide film to form an N-type heavily doped region;

[0012] Using the patterned gate electrode as a mask, etching the gate insulating layer on the N-type heavily doped region;

[0013] Metal is deposited on the N-type heavily doped region to form source and drain electrodes, and annealing is performed to obtain an oxide thin film transistor.

[0014] Optionally, an oxide film is formed on the buffer layer by atomic layer deposition, wherein the deposition temperature is not less than 150°C.

[0015] Optionally, the oxide film is any one of zinc oxide, indium gallium oxide, indium zinc oxide, indium gallium zinc oxide and indium tin zinc oxide films.

[0016] Optionally, the patterned oxide film is annealed, wherein: the annealing atmosphere is air or oxygen, and the annealing temperature is 300°C to 600°C.

[0017] Optionally, the gate insulating layer is made of any one of aluminum oxide, hafnium oxide and silicon oxide.

[0018] Optionally, the gate electrode is any one of metal molybdenum, metal nickel, metal tungsten and ITO film.

[0019] Optionally, ion implantation is performed on both ends of the oxide film to form an N-type heavily doped region, wherein the ions are any one of germanium, boron, arsenic, phosphorus and fluorine.

[0020] Optionally, the source and drain electrodes are any one of metal molybdenum, metal nickel, metal tungsten and ITO film.

[0021] Optionally, the source-drain electrodes are formed and annealed, wherein: the annealing atmosphere is air or oxygen, and the annealing temperature is 300° C. to 600° C.

[0022] According to another aspect of the present invention, there is provided an oxide thin film transistor, the transistor being manufactured by using the above-mentioned method for manufacturing an oxide thin film transistor, the transistor comprising:

[0023] a substrate having a buffer layer;

[0024] An oxide film, located on the buffer layer, wherein the oxide film is formed by atomic layer deposition, wherein both ends of the oxide film are N-type heavily doped regions formed by ion implantation, and the middle is an undoped region;

[0025] A gate insulating layer, located above the middle of the oxide film;

[0026] Source and drain electrodes are located above the N-type heavily doped regions at both ends of the oxide film;

[0027] A gate electrode is located on the gate insulating layer.

[0028] Compared with the prior art, the present invention has at least one of the following beneficial effects:

[0029] The present invention forms an oxide film by atomic layer deposition, and can precisely control the ratio of different elements by regulating the number of cycles of different element precursors, thereby achieving precise control of the electrical properties of the film, with high film quality and good repeatability. In addition, the self-limited film growth mechanism of the atomic layer deposition process surface can greatly improve the uniformity and uniformity of the film, making it easy to realize the preparation of ultra-large area oxide thin film transistor devices and circuits. The top-gate oxide thin film transistor prepared by the present invention can be used for more applications such as DRAM.

[0030] The present invention obtains an N-type heavily doped region by ion implantation. The ion implantation method can make oxygen vacancy defects exist stably, and will not re-combine with oxygen under high temperature conditions to cause failure of the heavily doped region, thus overcoming the thermal stability problem caused by hydrogen diffusion or plasma treatment in the traditional manufacturing process. In addition, the precursor of atomic layer deposition contains water source, which will introduce a certain amount of hydrogen elements into the film, affecting the electrical properties of the device such as bias stability. The use of ion implantation to form an N-type heavily doped region can not only enhance conductivity, but also reduce the influence of hydrogen elements in atomic layer deposition technology to a certain extent. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Other features, objects and advantages of the present invention will become more apparent from the detailed description of non-limiting embodiments made with reference to the following drawings:

[0032] Figure 1 is a schematic cross-sectional view of a substrate with a buffer layer in one embodiment of the present invention;

[0033] Figure 2 It is a schematic cross-sectional view of an embodiment of the present invention after an oxide film is formed on a buffer layer by atomic layer deposition;

[0034] Figure 3 is a schematic cross-sectional view of a gate insulating layer deposited on an oxide film in one embodiment of the present invention;

[0035] Figure 4 is a schematic cross-sectional view of a gate electrode deposited on a gate insulating layer in one embodiment of the present invention;

[0036] Figure 5 It is a schematic cross-sectional view of an embodiment of the present invention after boron ions are implanted to form an N-type heavily doped region;

[0037] Figure 6 It is a schematic cross-sectional view after etching the gate insulating layer on the N-type heavily doped region in one embodiment of the present invention;

[0038] Figure 7 It is a schematic cross-sectional view of depositing source and drain electrodes on the N-type heavily doped region in one embodiment of the present invention.

[0039] The corresponding reference numerals are: 101 - substrate, 102 - buffer layer, 103 - oxide film, 104 - gate insulating layer, 105 - gate electrode, 106 - N-type heavily doped region, 107 - source and drain electrodes. DETAILED DESCRIPTION

[0040] The present invention is described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several variations and improvements may be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.

[0041] An embodiment of the present invention provides a method for manufacturing an oxide thin film transistor. Figure 1-Figure 7 , the method comprising:

[0042] S1, providing a substrate 101 having a buffer layer 102, and forming an oxide thin film 103 on the buffer layer 102 by atomic layer deposition;

[0043] S2, performing photolithography and wet etching on the oxide film 103 in sequence to obtain a patterned oxide film 103;

[0044] S3, annealing the patterned oxide film 103;

[0045] S4, depositing a gate insulating layer 104 on the patterned oxide film 103 after annealing;

[0046] S5, depositing a gate electrode 105 on the gate insulating layer 104, and patterning the gate electrode 105 to form a patterned gate electrode 105, which is located in the middle of the gate insulating layer 104;

[0047] S6, using the patterned gate electrode 105 as a mask, ion implantation is performed on both ends of the oxide film 103 to form an N-type heavily doped region 106;

[0048] S7, using the patterned gate electrode 105 as a mask, etching the gate insulating layer 104 on the N-type heavily doped region 106 to remove the gate insulating layer 104 on the surface of the N-type heavily doped region 106;

[0049] S8. Deposit metal on the N-type heavily doped region 106 to form source and drain electrodes 107, and perform annealing to obtain an oxide thin film transistor.

[0050] Atomic layer deposition (ALD) is a method of forming a single-layer film on the surface of a substrate by alternating adsorption reactions of gas-phase precursor molecules. Each precursor molecule is deposited one by one in the reaction chamber through surface reactions. The process is roughly as follows:

[0051] Step 1, Precursor 1 (A Precursor) injection: First, a first precursor molecule (e.g., a metal precursor, such as an organic compound of aluminum) is injected into the reaction chamber so that it is adsorbed on the active sites on the substrate surface;

[0052] Step 2, removal of residual gas from precursor 1: exhausting the unadsorbed precursor 1 and some by-products from the reaction chamber, usually through a gas vacuum system;

[0053] Step 4, Precursor 2 (B Precursor) injection: Next, the second precursor molecule is injected into the reaction chamber;

[0054] Step 5, reaction of precursor 2: Precursor 2 reacts with the adsorbed precursor 1 sites to form a thin film of one atomic layer;

[0055] Step 6: Removal of residual gas from precursor 2: discharge the unreacted precursor 2 and reaction by-products from the reaction chamber.

[0056] Exemplarily, precursor 1 is trimethylaluminum, precursor 2 is water vapor, and the above 6 steps are repeated to finally obtain an aluminum oxide film.

[0057] Taking aluminum oxide as an example, in aluminum oxide deposition, each small cycle includes X injections of precursor 1 and Y injections of precursor 2. The entire ALD process consists of several small cycles. By adjusting the ratio of X to Y, the atomic ratio in aluminum oxide can be adjusted. The quality and electrical properties of oxide films are closely related to their atomic ratios. ALD can achieve precise control of material composition by depositing atoms layer by layer, obtain excellent film quality, and thus ensure its electrical properties.

[0058] The oxide thin film transistor in the embodiment of the present invention adopts a top gate self-aligned structure to reduce parasitic capacitance. The oxide film 103 is formed by atomic layer deposition, and the proportion of different elements can be accurately controlled by regulating the number of cycles of different element precursors (such as indium, zinc, gallium, and oxidants such as water vapor in the deposition process of indium gallium zinc oxygen film), so as to achieve precise control of the electrical properties of the film, and the film formation quality is high and the repeatability is good. In addition, the self-limited film growth mechanism of the atomic layer deposition process can greatly improve the uniformity and uniformity of the film, which is convenient for the preparation of oxide thin film transistor devices and circuits with ultra-large areas. The top gate oxide thin film transistor prepared by the present invention can be oriented to more applications such as DRAM. The embodiment of the present invention obtains the N-type heavily doped region 106 by ion implantation. The ion implantation method can make the oxygen vacancy defects exist stably, and will not re-combine with oxygen under high temperature conditions to cause the heavily doped region to fail, overcoming the thermal stability problem caused by hydrogen diffusion or plasma treatment in the traditional manufacturing process. In addition, the precursor of atomic layer deposition contains water, which will introduce a certain amount of hydrogen into the film, affecting the electrical properties of the device such as bias stability. The N-type heavily doped region 106 is formed by ion implantation. In addition to enhancing conductivity, it can also reduce the influence of hydrogen in the atomic layer deposition technology to a certain extent, thereby improving the electrical properties of the device.

[0059] During the film growth process, different materials may have different thermal expansion coefficients and lattice parameters, resulting in stress accumulation and film mismatch. The buffer layer can reduce the transmission of such stress and reduce the stress of the film during growth. In step S1, before forming the oxide film 103, the substrate 101 and the buffer layer 102 are cleaned, illustratively, by ultrasonic cleaning with acetone and isopropanol to provide a clean environment for subsequent film growth.

[0060] In some embodiments, the oxide film 103 is formed on the buffer layer 102 by atomic layer deposition, wherein the deposition temperature is not less than 150° C., so that the quality of the oxide film 103 meets the requirements of DRAM applications.

[0061] The oxide transistor prepared in the embodiment of the present invention is for display and DRAM applications, which require the transistor to have a higher switching ratio, lower leakage, larger on-state current and better subthreshold slope. In some embodiments, the oxide film 103 is any one of zinc oxide, indium gallium oxide, indium zinc oxide, indium gallium zinc oxide and indium tin zinc oxide films, which can better meet the above requirements of the transistor.

[0062] The oxide film 103 formed by atomic layer deposition inevitably has film defects, including oxygen vacancies, oxygen defects and oxide interface defects. In some embodiments, in step S3, a rapid thermal annealing furnace is used to anneal the patterned oxide film 103. The annealing atmosphere is air or oxygen, and the annealing temperature is 300°C to 600°C, so as to repair the above-mentioned film defects inside the film and on the interface, reduce the defect density, and improve the electrical quality and stability of the film.

[0063] A gate insulating layer with a high dielectric constant helps reduce capacitance and reduces the need for gate voltage. In addition, the interface quality between the gate insulating layer and the oxide film directly affects the electrical characteristics of the transistor. In some embodiments, in step S4, the material of the gate insulating layer 104 is any one of aluminum oxide, hafnium oxide, and silicon oxide, so that the gate insulating layer 104 has a higher dielectric constant and obtains a high-quality interface with the oxide film.

[0064] In some embodiments, in step S5 , the gate electrode 105 is any one of metal molybdenum, metal nickel, metal tungsten and ITO film, so that the gate electrode 105 has good conductivity and can ensure the interface quality between it and the gate insulating layer 104 .

[0065] In some embodiments, in step S6, ion implantation is performed on both ends of the oxide film 103 to form an N-type heavily doped region 106, wherein the ions are any one of germanium, boron, arsenic, phosphorus and fluorine, and the N-type heavily doped region 106 and the oxide film region in the middle that is not implanted are obtained. Thus, the conductivity of the implanted region can be improved, the contact resistance between the implanted region and the source and drain electrode 107 can be ensured to be small, the contact can be optimized, and the electrical performance of the transistor can be improved, and the cost is low.

[0066] In some other implementations, other types of ions may be implanted to form an N-type heavily doped region, as long as the same function as described above can be achieved.

[0067] In some embodiments, in step S8 , the source-drain electrode 107 is any one of metal molybdenum, metal nickel, metal tungsten and ITO film, so that the source-drain electrode 107 has good conductivity and ensures a small contact resistance between the source-drain electrode 107 and the oxide film 103 .

[0068] In some embodiments, the source-drain electrode 107 is annealed, wherein the annealing atmosphere is air or oxygen and the annealing temperature is 300° C. to 600° C. to improve the switching ratio, on-state current, subthreshold slope, leakage and other electrical properties of the transistor.

[0069] Another embodiment of the present invention provides an oxide thin film transistor, which is manufactured using the above-mentioned method for manufacturing an oxide thin film transistor. Figure 1-Figure 7 The transistor includes a substrate 101, an oxide film 103, a gate insulating layer 104, a source-drain electrode 107 and a gate electrode 105. The substrate 101 has a buffer layer 102; the oxide film 103 is located on the buffer layer 102, and the oxide film 103 is formed by atomic layer deposition. The two ends of the oxide film 103 are N-type heavily doped regions 106 formed by ion implantation, and the middle is an undoped region; the gate insulating layer 104 is located above the middle position of the oxide film 103; the source-drain electrode 107 is located above the N-type heavily doped region 106 at the two ends of the oxide film 103; and the gate electrode 105 is located on the gate insulating layer 104.

[0070] In the above-mentioned embodiment of the present invention, the transistor adopts a top-gate self-aligned structure, which reduces parasitic capacitance, and uses an atomic layer deposition process to prepare an oxide thin film. The film components can be precisely controlled, the film quality is high and the film uniformity is good. Ion implantation is used to form an N-type heavily doped region, which has good thermal stability. Ion implantation can also weaken the influence of hydrogen elements in the atomic layer deposition technology and improve the electrical properties of the device.

[0071] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art can make various modifications or variations within the scope of the claims, which does not affect the essence of the present invention. The above preferred features can be used in any combination without conflicting with each other.

Claims

1. A method for manufacturing an oxide thin film transistor, characterized in that: include: Providing a substrate having a buffer layer, and forming an oxide thin film on the buffer layer by atomic layer deposition; sequentially performing photolithography and wet etching on the oxide film to obtain a patterned oxide film; annealing the patterned oxide film; depositing a gate insulating layer on the annealed patterned oxide film; Depositing a gate electrode on the gate insulating layer, and performing a patterning process on the gate electrode; Using the patterned gate electrode as a mask, ion implantation is performed on both ends of the oxide film to form an N-type heavily doped region; Using the patterned gate electrode as a mask, etching the gate insulating layer on the N-type heavily doped region; Metal is deposited on the N-type heavily doped region to form source and drain electrodes, and annealing is performed to obtain an oxide thin film transistor.

2. The method for manufacturing an oxide thin film transistor according to claim 1, characterized in that: An oxide film is formed on the buffer layer by atomic layer deposition, wherein the deposition temperature is not less than 150°C.

3. The method for manufacturing an oxide thin film transistor according to claim 1, characterized in that: The oxide film is any one of zinc oxide, indium gallium oxide, indium zinc oxide, indium gallium zinc oxide and indium tin zinc oxide films.

4. The method for manufacturing an oxide thin film transistor according to claim 1, wherein: The patterned oxide film is annealed, wherein the annealing atmosphere is air or oxygen and the annealing temperature is 300°C to 600°C.

5. The method for manufacturing an oxide thin film transistor according to claim 1, characterized in that: The material of the gate insulating layer is any one of aluminum oxide, hafnium oxide and silicon oxide.

6. The method for manufacturing an oxide thin film transistor according to claim 1, characterized in that: The gate electrode is any one of metal molybdenum, metal nickel, metal tungsten and ITO film.

7. The method for manufacturing an oxide thin film transistor according to claim 1, characterized in that: Ion implantation is performed on both ends of the oxide film to form an N-type heavily doped region, wherein the ions are any one of germanium, boron, arsenic, phosphorus and fluorine.

8. The method for manufacturing an oxide thin film transistor according to claim 1, characterized in that: The source-drain electrode is any one of metal molybdenum, metal nickel, metal tungsten and ITO film.

9. The method for manufacturing an oxide thin film transistor according to claim 1, wherein: The source-drain electrodes are formed and annealed, wherein the annealing atmosphere is air or oxygen and the annealing temperature is 300° C. to 600° C.

10. An oxide thin film transistor, characterized in that: Prepared by the method for manufacturing an oxide thin film transistor according to any one of claims 1 to 9, the transistor comprises: a substrate having a buffer layer; An oxide film, located on the buffer layer, wherein the oxide film is formed by atomic layer deposition, wherein both ends of the oxide film are N-type heavily doped regions formed by ion implantation, and the middle is an undoped region; A gate insulating layer, located above the middle of the oxide film; Source and drain electrodes are located above the N-type heavily doped regions at both ends of the oxide film; A gate electrode is located on the gate insulating layer.

Citation Information

Cited By

  • Metal oxide thin film transistor preparation method and metal oxide thin film transistor

    CN121815702A