Double-catalyst-layer slurry, cathode gas diffusion electrode, membrane electrode and preparation method
Through the dual-catalytic layer slurry design, the cathode proton-gas channel is constructed, which solves the problems of low catalyst utilization and phosphoric acid toxicity in traditional high-temperature proton exchange membrane fuel cells, and achieves higher battery performance and life.
Patent Information
- Application Number
- CN202411032608.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-22
AI Technical Summary
In traditional high-temperature proton exchange membrane fuel cells, the catalyst deactivation caused by slow kinetics of oxygen reduction reaction and phosphoric acid adsorption leads to low catalyst utilization, and the toxicity of phosphoric acid on the active sites of the catalyst and the blockage of mass transfer channels, affecting battery performance and life.
The dual-catalytic layer slurry design is adopted, and the components and dispersion sequence of the outer and inner catalytic layers are regulated to build a cathode proton-gas channel, control the uniform distribution of phosphoric acid, and build a sufficient gas transmission channel to improve the catalyst utilization rate.
It improves the utilization rate of catalysts, optimizes the distribution of phosphoric acid and oxygen, reduces mass transfer resistance, and improves battery performance and life.
Smart Images

Figure CN119008972A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of high-temperature proton exchange membrane fuel cells, and in particular relates to a double-catalytic layer slurry, a cathode gas diffusion electrode, a membrane electrode, a high-temperature proton exchange membrane fuel cell and a preparation method thereof. Background Art
[0002] Proton exchange membrane fuel cells (PEMFCs) are considered to be the next generation of promising power sources due to their high energy conversion efficiency, high power density, no pollutant emissions, and relatively simple design. According to the operating temperature, PEMFCs are divided into low-temperature PEMFCs (LT-PEMFCs) based on Nafion membranes and high-temperature PEMFCs (HT-PEMFCs) based on polybenzimidazole (PBI) membranes doped with phosphoric acid (PA).
[0003] Nowadays, HT-PEMFCs operating at temperatures up to 200 °C have attracted widespread attention due to their high tolerance to impurities, faster electrode reaction kinetics, large amounts of reusable thermal energy, and simplified water management. However, due to the sluggish kinetics of the oxygen reduction reaction (ORR) and catalyst deactivation due to PA adsorption, a large amount of platinum catalyst must be used on the cathode to ensure satisfactory performance. This leads to a serious high cost problem and is the main obstacle to the commercialization of HT-PEMFC. Therefore, improving the utilization efficiency of platinum and improving the performance of HT-PEMFC is expected to promote its development.
[0004] The traditional cathode single catalyst layer (SCL) used in high-temperature proton exchange membranes is to coat the same catalyst slurry on the GDL (gas diffusion layer). Although the overall distribution of the catalyst layer structure is relatively uniform, it also causes the catalyst to be flooded due to the relatively high acid content on the side close to the PEM (proton exchange membrane), reducing the active sites of the catalyst; and on the side close to the GDL, the diffusion of phosphoric acid outward increases the difficulty of air or oxygen diffusion, greatly increasing the mass transfer resistance, and greatly affecting the performance and life of high-temperature proton exchange membrane fuel cells. Compared with other types of fuel cells, since there is no liquid water in HT-PEMFC, the more viscous phosphoric acid acts as a proton conductor, and the coverage and poisoning of phosphoric acid on the active sites of the catalyst are more serious. Summary of the invention
[0005] In order to solve the problem of low catalyst utilization in the catalyst layer of traditional high-temperature proton exchange membrane fuel cells due to phosphoric acid poisoning the active sites of the catalyst and blocking the mass transfer channels during battery operation, the inventors have conducted intensive research and provided a double catalyst layer slurry, a cathode gas diffusion electrode, a membrane electrode and a preparation method. By regulating the components and dispersion sequence of the double catalyst layer slurry, a HT-PEMFC catalyst layer structure with a cathode proton-gas channel is designed, the phosphoric acid is controlled to be evenly distributed in the catalyst layer, and sufficient gas transmission channels are constructed at the same time to improve the utilization of the catalyst and adapt to the high-temperature phosphoric acid environment.
[0006] The technical solution provided by the present invention is as follows:
[0007] In a first aspect, a double catalyst layer slurry for a cathode gas diffusion electrode comprises an outer catalyst layer slurry and an inner catalyst layer slurry;
[0008] The outer catalyst layer slurry includes a first catalyst, an ionomer, a binder and a first pore former;
[0009] The inner catalyst layer slurry includes a second catalyst, a binder, an ionomer and a second pore former;
[0010] The first catalyst is a carbon-supported Pt-based catalyst;
[0011] The first pore-forming agent is ethylene glycol and / or polyethylene glycol;
[0012] The second catalyst is Pt black and / or a carbon-supported Pt-based catalyst;
[0013] The second pore-forming agent is ethylene glycol and / or polyethylene glycol;
[0014] The ionomer in the outer catalyst layer slurry and the inner catalyst layer slurry is at least one of meta-fully aromatic polybenzimidazole, aromatic ether polybenzimidazole, fluorine-containing polybenzimidazole or 2,3,5,6-tetrafluorostyrene-4-phosphonic acid;
[0015] The binder in the outer catalyst layer slurry and the inner catalyst layer slurry is at least one of polytetrafluoroethylene, polyvinylidene fluoride, tetrafluoroethylene-hexafluoropropylene copolymer, ethylene chlorotrifluoroethylene copolymer, ethylene-tetrafluoroethylene copolymer, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer or polydimethylsiloxane.
[0016] In a second aspect, a method for preparing a double catalytic layer slurry for a cathode gas diffusion electrode comprises:
[0017] Preparation of outer catalyst layer slurry:
[0018] uniformly dispersing the first catalyst in a solvent to obtain a first catalyst solution;
[0019] Adding the ionomer solution dropwise to the first catalyst solution system and dispersing the solution uniformly to obtain the first catalyst system coated with the ionomer;
[0020] Continue to drop the binder into the above system, evenly disperse it, separate the solid from the liquid, and dry the solid to obtain the cathode outer layer catalyst;
[0021] Dispersing the cathode outer layer catalyst in a solvent, adding a first pore-forming agent, and fully dispersing the catalyst to obtain an outer catalyst layer slurry;
[0022] Preparation of inner catalyst layer slurry:
[0023] uniformly dispersing the second catalyst in the solvent to obtain a second catalyst solution;
[0024] Adding a binder dropwise into the second catalyst solution and dispersing the binder uniformly to obtain a second catalyst system having a binder network structure;
[0025] Continue to drop the ionomer solution into the above system, disperse it evenly, separate the solid from the liquid, and dry the solid to obtain the cathode inner layer catalyst;
[0026] After the cathode inner layer catalyst is dispersed in the solvent, a second pore-forming agent is added to the solution and fully dispersed to form an inner catalyst layer slurry.
[0027] In a third aspect, a method for preparing a cathode gas diffusion electrode having a double catalytic layer comprises:
[0028] The outer catalyst layer slurry and the inner catalyst layer slurry are prepared by the preparation method of the double catalyst layer slurry described in the second aspect;
[0029] After the outer catalyst layer slurry is fully dispersed, it is coated on the surface of the cathode gas diffusion layer and heated under an inert atmosphere to evaporate the first pore-forming agent to form pores, thereby forming the cathode outer catalyst layer;
[0030] After the inner catalyst layer slurry is fully dispersed, it is coated on the surface of the outer catalyst layer and heated under an inert atmosphere to evaporate the second pore-forming agent to form pores, thereby forming the cathode inner catalyst layer.
[0031] In a fourth aspect, a cathode gas diffusion electrode (cathode GDE) having a double catalytic layer is prepared by the preparation method of the cathode gas diffusion electrode having a double catalytic layer described in the third aspect.
[0032] In a fifth aspect, a membrane electrode comprises the cathode gas diffusion electrode with a double catalytic layer as described in the fourth aspect, a proton exchange membrane and an anode gas diffusion electrode, wherein the proton exchange membrane is a phosphoric acid-doped PBI membrane.
[0033] In a sixth aspect, a high temperature proton exchange membrane fuel cell (HT-PEMFC) comprises the membrane electrode described above; the operating temperature of the high temperature proton exchange membrane fuel cell is 140°C to 220°C.
[0034] A double catalytic layer slurry, a cathode gas diffusion electrode, a membrane electrode and a preparation method provided by the present invention have the following beneficial effects:
[0035] (1) The present invention changes the catalyst pretreatment method and reconstructs the distribution mode of the ionomer and binder on the catalyst surface, and prepares a catalyst (cathode inner layer catalyst) in which the ionomer gap is dispersed in the binder network and a catalyst (cathode outer layer catalyst) in which the binder gap is dispersed in the ionomer film defects. For the inner catalyst layer close to the proton exchange membrane, a catalyst in which the ionomer gap is dispersed in the binder network is used, and for the outer catalyst layer far from the proton exchange membrane, a catalyst in which the binder gap is dispersed in the ionomer film defects is used. Among them, the catalyst in which the binder gap is dispersed in the ionomer film defects has strong hydrophobicity and less phosphoric acid adsorption on the surface, which is conducive to opening the mass transfer channel; while the catalyst in which the ionomer gap is dispersed in the binder network, the ionomer film on its surface makes the catalyst particles less hydrophobic, and it is easier to form a phosphoric acid liquid film on the surface, which helps phosphoric acid diffuse to the outer catalyst layer. The present invention constructs different distribution modes of ionomer and binder on the catalyst surface in the inner and outer catalyst layers, so that the distribution of phosphoric acid and oxygen at the cathode is more reasonable when the battery is running, so as to achieve the effect of improving battery performance and improving catalyst utilization.
[0036] At the same time, pore formers are used in the cathode outer catalyst layer and the cathode inner catalyst layer of the present invention to construct sufficient gas transmission channels, especially to construct gradient gas transmission channels with larger outer and smaller inner portions. On the GDL side where the oxygen concentration is higher and the gas flow rate is faster, the larger pore size of the outer catalyst layer can transport the gas to the active sites more quickly. On the side close to the phosphoric acid-doped PBI membrane, the smaller pore structure brings a larger specific surface area, exposing more active sites to contact with oxygen.
[0037] (2) In the present invention, ethylene glycol or polyethylene glycol is specially selected as a pore-forming agent when dispersing the pretreated catalyst particles to prepare the catalyst layer slurry. It can play the following three effects in actual operation: ① The pretreated catalyst particles contain a binder that is easily precipitated in an organic solvent and an ionomer that is easily precipitated in water, which are difficult to be dispersed. Since ethylene glycol or polyethylene glycol can act as a hydrogen bond acceptor, it breaks the polarity of water and has a significant effect on the dispersibility and stability of the catalyst particles; ② By adjusting the molecular weight of polyethylene glycol, a catalyst layer with different pore sizes can be constructed; ③ By adjusting the content of ethylene glycol or polyethylene glycol, the porosity of the catalyst layer, that is, the number of pores, can be adjusted. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 This is a schematic diagram of the microstructure of the double-catalytic layer catalyst pretreatment of the cathode of the high-temperature proton exchange membrane fuel cell of the present invention, a is a catalyst in which the ionomer gaps are dispersed in the binder network (cathode inner layer catalyst), and b is a catalyst in which the binder gaps are dispersed in the defects of the ionomer film (cathode outer layer catalyst).
[0039] Figure 2 These are the membrane electrode polarization characteristic curves of Examples 1-2 of the present invention and Comparative Examples 1-2.
[0040] Figure 3 The membrane electrode impedance diagrams of Examples 1-2 and Comparative Examples 1-2 of the present invention are shown. DETAILED DESCRIPTION
[0041] The following detailed description of the present invention will make the features and advantages of the present invention more clear and explicit.
[0042] The word “exemplary” is used exclusively herein to mean “serving as an example, example, or illustration.” Any embodiment described herein as “exemplary” is not necessarily to be construed as preferred or advantageous over other embodiments.
[0043] The present invention provides a method for preparing a cathode gas diffusion electrode with a double catalytic layer, wherein the double catalytic layer is formed on the surface of the cathode gas diffusion layer and comprises a cathode outer catalytic layer and a cathode inner catalytic layer;
[0044] 1. Preparation of cathode outer catalytic layer
[0045] S1.1, uniformly dispersing the first catalyst in a solvent to obtain a first catalyst solution.
[0046] In this step, the first catalyst is one or more of Pt / C, PtFe / C or PtCo / C; in Pt / C, PtFe / C or PtCo / C, the mass fraction of Pt is 5wt.% to 70wt.%.
[0047] In this step, the solvent is water, alcohol or a polar aprotic solvent (such as N,N-dimethylacetamide DMAc, N,N-dimethylformamide DMF, N-methylpyrrolidone NMP or dimethyl sulfoxide DMSO).
[0048] S1.2, dropwise adding the ionomer solution into the first catalyst solution system, uniformly dispersing the ionomer, and forming a film on the first catalyst to obtain the first catalyst system coated with the ionomer.
[0049] In this step, the ionomer is an ionic polymer capable of absorbing phosphoric acid or conducting protons, and is meta-fully aromatic polybenzimidazole (mPBI), aromatic ether polybenzimidazole (OPBI), fluorinated polybenzimidazole (Fx At least one of PBI and 2,3,5,6-tetrafluorophenylethylene-4-phosphonic acid (PWN); x In PBI, x represents the atomic ratio of F, and the value of x is 1 to 8, preferably 4 to 6. Due to the film-forming property of the ionomer, the added ionomer solution will coat the surface of the first catalyst, that is, form a film on the surface of the first catalyst.
[0050] In this step, the mass ratio of the ionomer to the carbon carrier in the first catalyst is (10-50):100.
[0051] S1.3, add a binder dropwise to the first catalyst system coated with an ionomer and disperse it evenly so that the binder is dispersed in the first catalyst coated with an ionomer (the binder will be dispersed in the defects of the ionomer film), and obtain a cathode outer layer catalyst through solid-liquid separation and solid drying. In the cathode outer layer catalyst, the hydrophilic ionomer is located in the inner layer and the hydrophobic binder is located in the outer layer, which is an endophilic-exophobic catalyst.
[0052] In this step, the binder is a hydrophobic binder, including at least one of polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), ethylene chlorotrifluoroethylene copolymer (ECTFE), ethylene-tetrafluoroethylene copolymer (ETFE), tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA), and polydimethylsiloxane (PDMS).
[0053] In this step, the mass ratio of the binder to the carbon carrier in the first catalyst is (10-50):100.
[0054] The specific steps of S1.1 to S1.3 may be: dispersing the first catalyst in a solvent to obtain a first catalyst solution; then slowly dripping the ionomer solution, ultrasonicating for 5 minutes to 60 minutes, to obtain a first catalyst system coated with an ionomer; further dripping a binder and stirring and dispersing to allow the components in the slurry to fully contact, and finally filtering or centrifuging the slurry, and drying the solid to obtain a cathode outer layer catalyst.
[0055] S1.4, dispersing the cathode outer layer catalyst in a solvent, adding a first pore-forming agent, and fully dispersing the catalyst to obtain an outer catalyst layer slurry.
[0056] In this step, the first pore-forming agent is ethylene glycol and / or polyethylene glycol, preferably the molecular weight of polyethylene glycol is 600-1000, and the mass percentage of the first pore-forming agent is 30%-50% based on the total solid mass in the outer catalyst layer slurry.
[0057] In this step, the solvent is water, alcohol or a polar aprotic solvent (such as N,N-dimethylacetamide DMAc, N,N-dimethylformamide DMF, N-methylpyrrolidone NMP or dimethyl sulfoxide DMSO).
[0058] S1.5, after the outer catalyst layer slurry is fully dispersed, it is coated on the surface of the cathode gas diffusion layer (GDL), and heated at 50°C to 300°C under the protection of an inert atmosphere such as N2 to evaporate the first pore-forming agent to form pores, thereby forming the cathode outer catalyst layer.
[0059] 2. Preparation of cathode inner catalytic layer
[0060] S2.1, uniformly dispersing the second catalyst in a solvent to obtain a second catalyst solution.
[0061] In this step, the second catalyst is one or more of Pt black, PtCo / C or PtNi / C; in PtCo / C or PtNi / C, the mass content of Pt is 20wt.% to 70wt.%.
[0062] In this step, the solvent is water, alcohol or a polar aprotic solvent (such as N,N-dimethylacetamide DMAc, N,N-dimethylformamide DMF, N-methylpyrrolidone NMP or dimethyl sulfoxide DMSO).
[0063] S2.2, adding a binder dropwise to the second catalyst solution and dispersing the binder evenly to obtain a second catalyst system having a binder network structure.
[0064] The inventors found through SEM electron microscopy observation that the binder forms a network structure in the solvent and is entangled with the second catalyst, which is equivalent to providing a hydrophobic layer on the surface of the second catalyst.
[0065] In this step, the binder is a hydrophobic binder, including at least one of polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), ethylene chlorotrifluoroethylene copolymer (ECTFE), ethylene-tetrafluoroethylene copolymer (ETFE), tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA), and polydimethylsiloxane (PDMS).
[0066] In this step, the mass ratio of the binder to the carbon carrier in the second catalyst is (10-50):100. If Pt black is used as the second catalyst, the mass ratio of the binder to Pt black is (10-50):100.
[0067] S2.3, dropwise adding the ionomer solution to the second catalyst system having a binder network structure, uniformly dispersing the ionomer so that the ionomer is dispersed in the second catalyst having a binder network structure, separating the solid and the liquid, and drying the solid to obtain a cathode inner layer catalyst. In the cathode inner layer catalyst, the hydrophobic binder is located in the inner layer, and the hydrophilic ionomer is located in the outer layer, which is an endophobic-exophilic catalyst.
[0068] In this step, the ionomer is an ionic polymer capable of absorbing phosphoric acid or conducting protons, and is meta-fully aromatic polybenzimidazole (mPBI), aromatic ether polybenzimidazole (OPBI), fluorinated polybenzimidazole (F x At least one of PBI and 2,3,5,6-tetrafluorophenylethylene-4-phosphonic acid (PWN); x In PBI, x represents the atomic ratio of F, and the value of x is 1-8, preferably 4-6.
[0069] In this step, the mass ratio of the ionomer to the carbon carrier in the second catalyst is (10-50):100. If Pt black is used as the second catalyst, the mass ratio of the ionomer to Pt black is (10-50):100.
[0070] The specific steps of S2.1 to S2.3 may be: dispersing the second catalyst in a solvent to obtain a second catalyst solution; then slowly dropping a binder and dispersing by stirring to obtain a second catalyst system having a binder network structure; further dropping an ionomer solution, ultrasonicating for 5 minutes to 20 minutes to allow the components in the slurry to fully contact, and finally filtering or centrifuging the slurry, and drying the solid to obtain the cathode inner layer catalyst.
[0071] S2.4, after dispersing the cathode inner layer catalyst in the solvent, add the second pore-forming agent into the solution and fully disperse it to form an inner catalyst layer slurry.
[0072] In this step, the second pore former is ethylene glycol and / or polyethylene glycol, and preferably the molecular weight of polyethylene glycol is ≤ 600. Based on the total solid mass in the cathode inner catalyst layer slurry, the mass percentage of the second pore former is 0% to 30%.
[0073] In this step, the solvent is water, alcohol or a polar aprotic solvent (such as N,N-dimethylacetamide DMAc, N,N-dimethylformamide DMF, N-methylpyrrolidone NMP or dimethyl sulfoxide DMSO).
[0074] S2.5, after the inner catalyst layer slurry is fully dispersed, it is coated on the surface of the outer catalyst layer, and heated at 50°C to 300°C under the protection of an inert atmosphere such as N2 to evaporate the second pore-forming agent to form pores, thereby forming the cathode inner catalyst layer.
[0075] In the cathode double catalytic layer of the present invention, the regulation of the distribution of phosphoric acid by the inner and outer catalytic layers is mainly achieved by the distribution of the ionomer that adsorbs phosphoric acid and the binder that absorbs acid on the catalyst surface. For the outer catalytic layer that requires a gas channel more, the ionomer-coated catalyst powder with dispersed binder gaps is used in a targeted manner, and its hydrophobicity is strong, and the contact angle is 75° to 95° (preferably 80° to 90°); for the inner catalytic layer close to one side of the membrane, the ionomer-coated catalyst powder with dispersed binder gaps is used in a targeted manner, and its hydrophobicity is weak, and the contact angle is 45° to 65° (preferably 50° to 60°).
[0076] In the cathode double catalytic layer of the present invention, the construction of the gas channel of the inner and outer catalytic layers is mainly achieved by evaporating pores of pore formers, preferably pore formers of different molecular weights and contents. For the outer catalytic layer close to the GDL side, high molecular weight polyethylene glycol is used to produce a larger pore size. For the inner catalytic layer close to the membrane side, ethylene glycol or low molecular weight polyethylene glycol is used to obtain a smaller pore size. The gradient pore structure reduces the diffusion resistance of air in the catalytic layer. Of course, the outer catalytic layer close to the GDL side can also use ethylene glycol or low molecular weight polyethylene glycol. The pore formers in the inner and outer catalytic layers are consistent. At this time, the void structure in the inner and outer catalytic layers is consistent. The former scheme is preferred to obtain a gradient pore structure to achieve a better mass transfer effect. Furthermore, in the cathode outer catalytic layer and the cathode inner catalytic layer, the loading of precious metals is 0.05 to 2.0 mg cm -2 , and the precious metal loading in the inner catalytic layer of the cathode is not lower than the precious metal loading in the outer catalytic layer of the cathode.
[0077] The present invention reconstructs the distribution mode of ionomer and binder on the catalyst surface by changing the catalyst pretreatment means, and prepares catalysts (cathode inner layer catalysts) in which ionomer gaps are dispersed in the binder network and catalysts (cathode outer layer catalysts) in which binder gaps are dispersed in the defects of ionomer film. For the inner catalytic layer close to the proton exchange membrane, a catalyst in which ionomer gaps are dispersed in the binder network is used, and for the outer catalytic layer far away from the proton exchange membrane, a catalyst in which binder gaps are dispersed in the defects of ionomer film is used. Among them, the catalyst in which the binder gap is dispersed in the defects of ionomer film has strong hydrophobicity, less phosphoric acid adsorption on the surface, which is conducive to opening the mass transfer channel; while the catalyst in which ionomer gaps are dispersed in the binder network, the ionomer film on its surface makes the catalyst particles less hydrophobic, and it is easier to form a phosphoric acid liquid film on the surface, which assists phosphoric acid to diffuse to the outer catalytic layer. The present invention constructs different distribution modes of ionomer and binder on the catalyst surface in the inner and outer catalytic layers, so that the distribution of phosphoric acid and oxygen at the cathode is more reasonable when the battery is running, so as to achieve the effect of improving battery performance and improving catalyst utilization.
[0078] At the same time, pore formers are used in the cathode outer catalyst layer and the cathode inner catalyst layer of the present invention to construct sufficient gas transmission channels, especially to construct gradient gas transmission channels with larger outer and smaller inner portions. On the GDL side where the oxygen concentration is higher and the gas flow rate is faster, the larger pore size of the outer catalyst layer can transport the gas to the active sites more quickly. On the side close to the phosphoric acid-doped PBI membrane, the smaller pore structure brings a larger specific surface area, exposing more active sites to contact with oxygen.
[0079] The present invention also provides a cathode gas diffusion electrode (cathode GDE) with a double catalytic layer, which is prepared by the above-mentioned method for preparing the cathode gas diffusion electrode with a double catalytic layer.
[0080] The present invention also provides a membrane electrode, comprising the cathode gas diffusion electrode with double catalytic layers, a proton exchange membrane and an anode gas diffusion electrode as described above, wherein the proton exchange membrane is a phosphoric acid-doped PBI membrane.
[0081] The present invention also provides a high temperature proton exchange membrane fuel cell (HT-PEMFC), comprising the membrane electrode described above; the operating temperature of the high temperature proton exchange membrane fuel cell is 140°C to 220°C.
[0082] Example / Comparative Example
[0083] Example 1
[0084] A method for preparing a cathode gas diffusion electrode and a membrane electrode having a double catalytic layer comprises the following steps:
[0085] Preparation of gas diffusion layer (GDL): First, VulcanXC-72 carbon powder and PTFE emulsion were mixed, and an appropriate amount of ethanol was added. The slurry was prepared by ultrasonic stirring, and then applied to the surface of commercial Toray carbon paper. The carbon powder loading and PTFE content were determined by weighing. Finally, it was placed in a muffle furnace and heat treated at 340°C for 25 minutes. After cooling to room temperature, a gas diffusion layer was obtained, which was used as the anode gas diffusion layer and the cathode gas diffusion layer in the subsequent steps.
[0086] Preparation of anode GDE (anode catalyst layer + anode gas diffusion layer): weigh the required Pt / C catalyst (0.5 mgPt / cm 2 ), adding a small amount of deionized water to stir and moisten, then adding a certain amount of PTFE water-alcohol solution, and ultrasonically dispersing it to obtain an anode catalyst slurry; the anode catalyst slurry is evenly coated on the surface of the microporous layer of the anode gas diffusion layer by ultrasonic spraying to obtain an anode GDE.
[0087] Preparation of cathode outer layer catalyst: The catalyst PtCo / C (Pt content 30wt.%) was dispersed in the organic solvent NMP, and then the ionomer solution F6PBI (1wt.%) was slowly dripped into it and ultrasonicated for 40min. The binder PTFE was further dripped into it and dispersed by stirring (500r·min -1 , 30min) to allow the various components in the slurry to fully contact, and finally centrifuge the slurry (8000r·min -1 ), and drying the solid to obtain a cathode outer layer catalyst, the structure of which is as follows Figure 1 b. The catalyst particles have a strong hydrophobicity on the outer surface, a contact angle of 80° to 90°, and a total pore area of 60 to 90 m 2 / g, median pore size V200~800nm, average pore size 60~150nm, porosity 30%~45%, electrochemical active specific surface area 72.061m 2 ·g -1 The microscopic performance is that the binder gaps are dispersed in the defects of the ionomer film, and the two cover the catalyst surface. The mass ratio of the ionomer to the carbon carrier in the catalyst is 30%, and the mass ratio of the binder to the carbon carrier in the catalyst is 10%.
[0088] Preparation of cathode inner layer catalyst: The catalyst PtCo / C (Pt content 30wt.%) was dispersed in NMP, and then the binder PTFE was slowly dripped and dispersed by stirring, and the ionomer solution F6PBI (1wt.%) was further dripped and ultrasonicated for 5min to make the components in the slurry fully contact, and finally the slurry was centrifuged (8000r·min -1 ), and drying the solid to obtain a catalyst powder in which the ionomer is interstitially dispersed in the binder network, and the structure thereof is as follows Figure 1 As shown in a, its macroscopic performance is that the outer surface is weakly hydrophobic, the contact angle is 50° to 60°, and the total pore area is 30 to 50 m 2 / g, median pore size V100~150nm, average pore size 30~50nm, porosity 25%~30%, electrochemical active specific surface area 50.582m 2 ·g -1 The microscopic performance is that the ionomer is interspersed in the binder network, and the two cover the catalyst surface. Among them, the mass ratio of the ionomer to the carbon carrier in the catalyst is 10%, and the mass ratio of the binder to the carbon carrier in the catalyst is 30%.
[0089] Preparation of cathode GDE (cathode double catalytic layer + cathode gas diffusion layer):
[0090] The cathode outer layer catalyst is dispersed in NMP; based on the total solid mass in the outer catalyst layer slurry, 40wt.% of PEG600 is added, and after being fully dispersed, it is coated on the surface of the cathode gas diffusion layer, the solvent is evaporated at 120°C, and heated at 250°C for 3h to volatilize the pore-forming agent to form an outer catalyst layer; the cathode inner layer catalyst is dispersed in NMP; based on the total solid mass in the cathode inner catalyst layer slurry, 5wt.% of PEG400 is added, and after being fully dispersed, it is coated on the outer catalyst layer, the solvent is evaporated at 120°C, and heated at 250°C for 3h to volatilize the pore-forming agent to form an inner catalyst layer.
[0091] Preparation of PBI / H3PO4 composite membrane by immersion method: S1, cut the PBI membrane into a certain size as needed; S2, soak the cut membrane in 85wt.% phosphoric acid at 120℃; S3, use filter paper to absorb the excess phosphoric acid on the membrane surface, weigh it quickly, and obtain the phosphoric acid adsorption capacity of the membrane. The mass ratio of phosphoric acid to PBI is used to examine the phosphoric acid adsorption capacity of the membrane. PA / m PBI The cycle S2→S3 was repeated until the phosphoric acid adsorption amount reached 400 wt.%.
[0092] The prepared electrodes and the PBI / H3PO4 composite membrane are stacked in sequence in a mold, that is, the anode GDE and the cathode GDE are located on both sides of the PBI / H3PO4 composite membrane, and the cathode inner catalyst layer is adjacent to the PBI / H3PO4 composite membrane. Then, the membrane electrode is placed in a hot press for hot pressing and molding to obtain a fuel cell membrane electrode, which is then placed in a sealed bag for storage.
[0093] The active area of the membrane electrode prepared in this example is 50 cm 2 The composition and structure of the cathode and anode gas diffusion layers are the same, both consisting of a support layer and a microporous layer. The support layer is mainly Torray carbon paper with a thickness of 140 μm. The microporous layer is mainly composed of carbon powder and PTFE. The type of carbon powder is Vulcan XC-72, and the carbon powder loading in the microporous layer is 4 mg cm -2 The anode catalyst layer is composed of 40wt.% Pt / C catalyst (40wt.% is the percentage of Pt mass in Pt / C catalyst to the total mass of catalyst) and PTFE, and the platinum loading is 0.5mg·cm -2 The content of PTFE in the anode catalyst layer is 20wt.%. The cathode catalyst layer is composed of 30% PtCo / C, PTFE, and F6PBI, and the Pt loading is 0.5mg·cm -2 (The inner and outer catalyst layers are both 0.25 mg cm -2), the cathode catalytic layer includes an inner cathode catalytic layer and an outer cathode catalytic layer, the inner cathode catalytic layer is close to the proton exchange membrane, and the mass ratio of F6PBI to the carbon carrier in the catalyst is 10%, and the mass ratio of PTFE to the carbon carrier in the catalyst is 30%; the outer cathode catalytic layer is close to the microporous layer, and the mass ratio of F6PBI to the carbon carrier in the catalyst is 30%, and the mass ratio of PTFE to the carbon carrier in the catalyst is 10%.
[0094] Example 2
[0095] This embodiment 2 is the same as embodiment 1, with the only difference being that PEG400 is used as the pore-forming agent for the inner and outer catalytic layers of the cathode, and the mass percentage of the pore-forming agent is 20% based on the total solid mass in the outer catalytic layer slurry; and the mass percentage of the pore-forming agent is 20% based on the total solid mass in the inner catalytic layer slurry.
[0096] Comparative Example 1
[0097] The comparative example 1 is the same as the example 2, and the only difference is that the cathode outer catalytic layer in the example 2 is used as the cathode inner catalytic layer of the comparative example 1, and the cathode inner catalytic layer in the example 2 is used as the cathode outer catalytic layer of the comparative example 1.
[0098] Comparative Example 2
[0099] Comparative Example 2 is the same as Example 1, except that no pore former is used in the preparation of cathode GDE (cathode double catalytic layer + cathode gas diffusion layer).
[0100] Performance Testing
[0101] With reference to GB / T 20042.5-2009, the polarization curve test of the obtained high-temperature proton exchange membrane fuel cell membrane electrode was carried out, and the specific operating conditions were: the single cell operating temperature was 160°C, the anode was fed with pure hydrogen, the cathode was fed with atmospheric pressure air, and the cathode / anode feeds were 3 / 1.5 times the stoichiometric ratio, respectively.
[0102] According to GB / T 20042.5-2009, the membrane electrode impedance of high-temperature proton exchange membrane fuel cell was tested. The specific operating conditions were: the single cell operating temperature was 160°C, the anode was fed with pure hydrogen, the cathode was fed with atmospheric pressure air, the cathode / anode feed was 3 / 1.5 times the stoichiometric ratio, and the discharge current density was 0.5A·cm -2 .
[0103] With reference to GB / T 20042.5-2009, high-temperature proton exchange membrane fuel cell membrane electrode cyclic voltammetry was carried out. The specific operating conditions were: the single cell operating temperature was 160°C, and dry N2 was introduced into the cathode at a flow rate of 4.6 ml min -1 cm -2 ; Dry H2 was introduced into the anode at a flow rate of 6.9 ml min -1 cm -2 ; Voltage range is 0.05V-1.2V, scan rate is 0.05V·s -1 .
[0104] Test results see Figure 2-3 Example 1 is a membrane electrode with a cathode double catalytic layer constructed using gradient proton-gas channels, Example 2 is a membrane electrode with a cathode double catalytic layer constructed using gradient proton channels and uniform gas channels, Comparative Example 1 is a membrane electrode with a cathode double catalytic layer of reverse gradient proton channels and uniform gas channels, and Comparative Example 2 is a membrane electrode with a cathode double catalytic layer of gradient proton channels and no additional gas channels.
[0105] See also Figure 2 The membrane electrode polarization characteristic curves of the cathode structures of Examples 1 to 2 of the present invention and the cathode structures of Comparative Examples 1 to 2 are measured. Figure 2 It can be seen that at 0.1A·cm -2 Under the conditions of 0.5A·cm -2 Under the conditions of 1.0 A·cm -2 Under the conditions, the voltages of the membrane electrodes corresponding to the cathode structures prepared in Examples 1 to 2 of the present invention and the cathode structures prepared in Comparative Examples 1 to 2 were measured to be 0.512 V, 0.490 V, 0.385 V, and 0.469 V, respectively. The maximum power densities of the membrane electrodes corresponding to the cathode structures prepared in Examples 1 to 2 of the present invention and the cathode structures prepared in Comparative Examples 1 to 2 were measured to be 0.657 W·cm -2 、0.619W·cm -2 、0.396W·cm -2 、0.573W·cm -2 As can be seen from the above, compared with the membrane electrode with cathode structure prepared in Comparative Examples 1-2, the membrane electrode with cathode double catalytic layer with differential distribution of ionomer-binder in Examples 1-2 of the present invention has smaller polarization loss and higher maximum power density.
[0106] See also Figure 3 From the impedance spectrum, it can be seen that compared with comparative examples 1 to 2, embodiments 1 to 2 have smaller internal resistance at high frequencies and cathode charge transfer resistance at medium frequencies. This is mainly due to the fact that the binder gaps of the cathode outer catalyst layer are dispersed in the defects of the ionomer film, and this structure makes it easier to form a phosphoric acid liquid film on the catalyst surface inside the ionomer film; the ionomer gaps on the catalyst surface of the cathode inner catalyst layer are dispersed on the binder network. While this structure adsorbs phosphoric acid on the catalyst surface, the hydrophobic binder network further limits the aggregation of phosphoric acid, prevents excessive phosphoric acid from poisoning the active sites of the catalyst, and constructs an oxygen transmission channel. With the cooperation of the inner and outer catalyst layers of the cathode, the proton and oxygen transmission channels are reasonably regulated, thereby reducing cathode polarization and ohmic polarization and improving battery performance. The cathode double catalytic layer of Example 2 only has differences in the coating state of the binder and ionomer on the catalyst surface, but no gradient changes in the pore structure, i.e., the oxygen transmission channel, so the improvement effect on cathode polarization is relatively limited, but compared with comparative examples 1 to 2, there is still a significant reduction in polarization. In Comparative Example 1, the cathode outer catalyst layer uses surface ionomer-coated acid-philic catalyst particles, which causes phosphoric acid to be adsorbed on the catalyst surface, blocking the channel for oxygen to be transferred to the inner catalyst layer, so that the catalyst in the inner catalyst layer cannot be fully utilized. In Comparative Example 2, its cathode impedance is larger than that of Example 1 with a similar structure, which is attributed to the increase in mass transfer polarization caused by the lack of gas transmission channels.
[0107] The present invention has been described in detail above in conjunction with specific implementations and exemplary examples, but these descriptions cannot be understood as limiting the present invention. Those skilled in the art understand that, without departing from the spirit and scope of the present invention, a variety of equivalent substitutions, modifications or improvements may be made to the technical solution of the present invention and its implementation methods, all of which fall within the scope of the present invention. The scope of protection of the present invention shall be subject to the attached claims.
[0108] The contents not described in detail in the specification of the present invention belong to the common knowledge of those skilled in the art.
Claims
1. A cathode double catalytic layer slurry, characterized in that: It includes an outer catalyst layer slurry and an inner catalyst layer slurry; The outer catalyst layer slurry includes a first catalyst, an ionomer, a binder and a first pore former; The inner catalyst layer slurry includes a second catalyst, a binder, an ionomer and a second pore former; The first catalyst is a carbon-supported Pt-based catalyst; The first pore-forming agent is ethylene glycol and / or polyethylene glycol; The second catalyst is Pt black and / or a carbon-supported Pt-based catalyst; The second pore-forming agent is ethylene glycol and / or polyethylene glycol; The ionomer in the outer catalyst layer slurry and the inner catalyst layer slurry is at least one of meta-fully aromatic polybenzimidazole, aromatic ether polybenzimidazole, fluorine-containing polybenzimidazole or 2,3,5,6-tetrafluorostyrene-4-phosphonic acid; The binder in the outer catalyst layer slurry and the inner catalyst layer slurry is at least one of polytetrafluoroethylene, polyvinylidene fluoride, tetrafluoroethylene-hexafluoropropylene copolymer, ethylene chlorotrifluoroethylene copolymer, ethylene-tetrafluoroethylene copolymer, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer or polydimethylsiloxane.
2. The cathode double catalytic layer slurry according to claim 1, characterized in that: The mass ratio of the ionomer in the outer catalyst layer slurry to the carbon carrier in the first catalyst is (10-50):100; and / or The mass ratio of the ionomer in the inner catalyst layer slurry to the carbon carrier in the second catalyst is (10-50):
100. If Pt black is used as the second catalyst, the mass ratio of the ionomer to Pt black is (10-50):
100.
3. The cathode double catalytic layer slurry according to claim 1, characterized in that: The mass ratio of the binder in the outer catalyst layer slurry to the carbon carrier in the first catalyst is (10-50):100; and / or The mass ratio of the binder in the inner catalyst layer slurry to the carbon carrier in the second catalyst is (10-50):
100. If Pt black is used as the second catalyst, the mass ratio of the binder to Pt black is (10-50):
100.
4. The cathode double catalytic layer slurry according to claim 1, characterized in that: Based on the total solid mass in the outer catalyst layer slurry, the mass percentage of the first pore-forming agent is 30% to 50%; and / or Based on the total solid mass in the inner catalyst layer slurry, the mass percentage of the second pore-forming agent is 0% to 30%.
5. A method for preparing a cathode double catalytic layer slurry according to any one of claims 1 to 4, characterized in that: include: Preparation of outer catalyst layer slurry: uniformly dispersing the first catalyst in a solvent to obtain a first catalyst solution; Adding the ionomer solution dropwise to the first catalyst solution system and dispersing the solution uniformly to obtain the first catalyst system coated with the ionomer; Continue to drop the binder into the above system, evenly disperse it, separate the solid from the liquid, and dry the solid to obtain the cathode outer layer catalyst; Dispersing the cathode outer layer catalyst in a solvent, adding a first pore-forming agent, and fully dispersing the catalyst to obtain an outer catalyst layer slurry; Preparation of inner catalyst layer slurry: uniformly dispersing the second catalyst in the solvent to obtain a second catalyst solution; Adding a binder dropwise into the second catalyst solution and dispersing the binder uniformly to obtain a second catalyst system having a binder network structure; Continue to drop the ionomer solution into the above system, disperse it evenly, separate the solid from the liquid, and dry the solid to obtain the cathode inner layer catalyst; After the cathode inner layer catalyst is dispersed in the solvent, a second pore-forming agent is added to the solution and fully dispersed to form an inner catalyst layer slurry.
6. The method for preparing the cathode double catalytic layer slurry according to claim 5, characterized in that: The solvent of the first catalyst solution is at least one of water, alcohol or polar aprotic solvent; and / or The solvent of the second catalyst solution is at least one of water, alcohol or a polar aprotic solvent.
7. A method for preparing a cathode gas diffusion electrode having a double catalytic layer, characterized in that: include: The outer catalyst layer slurry and the inner catalyst layer slurry are prepared by the method for preparing the cathode double catalyst layer slurry according to claim 5 or 6; After the outer catalyst layer slurry is fully dispersed, it is coated on the surface of the cathode gas diffusion layer and heated under an inert atmosphere to evaporate the first pore-forming agent to form pores, thereby forming the cathode outer catalyst layer; After the inner catalyst layer slurry is fully dispersed, it is coated on the surface of the outer catalyst layer and heated under an inert atmosphere to evaporate the second pore-forming agent to form pores, thereby forming the cathode inner catalyst layer.
8. A cathode gas diffusion electrode having a double catalytic layer, characterized in that: The cathode gas diffusion electrode having a double catalytic layer is prepared by the preparation method of claim 6.
9. A membrane electrode, characterized in that: Contains the cathode gas diffusion electrode with double catalytic layers, the proton exchange membrane and the anode gas diffusion electrode as claimed in claim 8, wherein the proton exchange membrane is a phosphoric acid-doped PBI membrane.
10. A high temperature proton exchange membrane fuel cell, characterized in that: A membrane electrode comprising the membrane electrode as claimed in claim 9.
Citation Information
Cited By
Dry-type preparation method and device for catalyst layer of high-temperature proton exchange membrane fuel cell
CN122202354A