Method for preparing modified NASICON type sodium ion solid electrolyte
By regulating the raw material ratio and synthesizing NZSP glass using molten water quenching process, the problems of sodium and phosphorus volatilization and high-temperature sintering in traditional sintering methods are solved, and high-performance NASICON oxide solid electrolyte is prepared at low temperatures, improving conductivity Rate and density enhance battery safety.
Patent Information
- Application Number
- CN202411255812.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-22
AI Technical Summary
The production cycle of NASICON type oxide solid electrolyte is long and the sintering temperature is high, which causes sodium and phosphorus elements to volatilize, generate ZrO2 heterophase, reduce ionic conductivity, and affect battery safety.
By regulating the raw material ratio of the initial sodium, silicon, zirconium and phosphorus sources, NZSP glass is synthesized by melting first and then water quenching, and NZSP glass is added as a sintering additive during the sintering process to reduce the sintering temperature and increase the sintering temperature. Density, alleviate grain boundary resistance, and improve the overall ionic conductivity of sodium ion solid electrolyte.
The NASICON type oxide solid electrolyte with excellent performance was prepared under low sintering temperature, which reduced the heterophasic content, improved the ionic conductivity and density, and enhanced the safety of the battery.
Smart Images

Figure CN119009083A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of sodium ion batteries, and in particular relates to a method for preparing a modified NASICON type sodium ion solid electrolyte. Background Art
[0002] One of the main issues limiting the practical application of sodium-ion batteries with non-aqueous liquid electrolytes is battery safety. The organic solvents used in these electrolytes are flammable, leaky, and have low thermal stability. In particular, the battery may explode when it is overcharged, short-circuited internally, or subjected to high temperatures, which can cause major safety issues. Solid-state electrolytes appear to be the most attractive option due to their excellent thermal and chemical stability.
[0003] Na 1+x Zr2Si x P 3-x O 12 (hereinafter referred to as NZSP) type oxide solid electrolyte was first discovered in 1976 and named NASICON. It has been favored by researchers because of its three-dimensional spatial structure for sodium ions to pass through and multiple ion substitution sites. It is one of the most promising sodium ion solid electrolytes. In NASICON-type solid electrolytes, material density, carrier concentration, crystal phase composition and structure are the main reasons affecting its performance. Grain resistance and grain boundary resistance jointly determine the ionic conductivity of the electrolyte body, and the grain boundary resistance is much larger than the grain resistance. Selecting appropriate doping elements at appropriate lattice positions of the main material for doping is an effective strategy to change the electrochemical properties of the material. Due to the different charges and ionic radii of the elements, doping will change the occupancy of the sodium ion sites, optimize the unit cell parameters, and affect the density of the sample. At the same time, it can effectively change the phase composition, regulate the grain boundary composition, improve the grain ion conductivity, and reduce the grain boundary resistance.
[0004] The preparation methods of NASICON oxide solid electrolytes include solid phase sintering, hydrothermal method, coprecipitation method, sol-gel method, hot pressing sintering, spark plasma sintering, etc. Among them, the solid phase sintering method has been widely used due to its advantages such as simple operation process, low raw material cost, and easy large-scale production. However, the traditional solid phase sintering method for preparing NASICON oxide solid electrolytes has a long production cycle and a high sintering temperature. In addition, under a long-term high temperature environment, the sodium and phosphorus elements in the NASICON oxide solid electrolyte will volatilize, generate ZrO2 impurity phase, and reduce ionic conductivity. Summary of the invention
[0005] In view of this, an object of the present invention is to provide a method for preparing a modified NASICON type sodium ion solid electrolyte, which can prepare a NASICON type oxide solid electrolyte material with excellent performance under a relatively low sintering temperature condition.
[0006] The present invention provides a method for preparing a modified NASICON type sodium ion solid electrolyte, comprising the following steps:
[0007] a) mixing a Na source compound, a Zr source compound, a Si source compound and a P source compound, ball milling, calcining, crushing, melting and water quenching to obtain NZSP glass;
[0008] In step a), based on the molar amounts of Na, Zr, Si and P, the molar ratio of the Na source compound, the Zr source compound, the Si source compound and the P source compound is (47-52):(11-14):(50-55):10;
[0009] b) mixing the Na source compound, the Zr source compound, the Si source compound, the P source compound and the NZSP glass, ball milling, calcining, crushing, pressing and sintering to obtain a modified NASICON type sodium ion solid electrolyte.
[0010] Preferably, in step a), based on the molar amounts of Na, Zr, Si and P, the molar ratio of the Na source compound, the Zr source compound, the Si source compound and the P source compound is 49:13.5:52:10.
[0011] Preferably, in step a), the Na source compound is Na2CO3; the Zr source compound is ZrO2; the Si source compound is SiO2; and the P source compound is NH4H2PO4.
[0012] Preferably, in step a), the calcination temperature is 750-1050° C. and the calcination time is 2-6 hours.
[0013] Preferably, in step a), the melting temperature is 1300-1550° C.; and the melting time is 2.5-5 h.
[0014] Preferably, in step b), the Na source compound is Na2CO3; the Zr source compound is ZrO2; the Si source compound is SiO2; and the P source compound is NH4H2PO4.
[0015] Preferably, in step b), based on the molar amounts of Na, Zr, Si and P, the molar ratio of the Na source compound, the Zr source compound, the Si source compound and the P source compound is (2.5-3.5):2:(1.5-2.5):(0.5-1.5).
[0016] Preferably, in step b), the NZSP glass accounts for 1-10% of the total mass of the Na source compound, the Zr source compound, the Si source compound, the P source compound and the NZSP glass.
[0017] Preferably, in step b), the calcination temperature is 750-1050° C. and the calcination time is 2-6 hours.
[0018] Preferably, in step b), the sintering temperature is 1000-1300° C.; and the sintering time is 6-10 hours.
[0019] Compared with the prior art, the present invention provides a method for preparing a modified NASICON type sodium ion solid electrolyte. The method provided by the present invention comprises the following steps: a) ball milling, calcining, crushing, melting, and water quenching of a Na source compound, a Zr source compound, a Si source compound, and a P source compound to obtain NZSP glass; in step a), the molar ratio of the Na source compound, the Zr source compound, the Si source compound, and the P source compound is (47-52): (11-14): (50-55): 10 based on the molar amount of Na, Zr, Si, and P; b) ball milling, calcining, crushing, pressing, and sintering of the Na source compound, the Zr source compound, the Si source compound, the P source compound, and the NZSP glass to obtain a modified NASICON type sodium ion solid electrolyte. The method provided by the present invention firstly adjusts the raw material ratio of the initial sodium source, silicon source, zirconium source and phosphorus source, and synthesizes NZSP glass with a relatively low melting temperature (800-950°C) by a process of first melting and then water quenching; then the glass is used as a sintering aid and added in the process of sintering to prepare a NASICON type sodium ion solid electrolyte; the glass liquid phase flowing at high temperature promotes the transfer of substances, which not only effectively reduces the sintering temperature, improves the density and reduces the impurity content, but also the sintering is also a process of heat treating the NZSP glass; the conductive crystalline phase sodium zirconium phosphate (NaZr2(PO4)3) formed by the heat treatment also has ionic conductivity, which is beneficial to the transmission of sodium ions at the grain boundaries, relieves the grain boundary resistance and improves the overall ionic conductivity of the sodium ion solid electrolyte material. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0021] Figure 1 is a scanning electron microscope image of the solid electrolyte material prepared in Comparative Example 1 of the present invention;
[0022] Figure 2 is a scanning electron microscope image of the solid electrolyte material prepared in Example 3 of the present invention;
[0023] Figure 3 3 is a scanning electron microscope image of the solid electrolyte material prepared in Example 4 of the present invention. DETAILED DESCRIPTION
[0024] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] The present invention provides a method for preparing a modified NASICON type sodium ion solid electrolyte, comprising the following steps:
[0026] a) mixing a Na source compound, a Zr source compound, a Si source compound and a P source compound, ball milling, calcining, crushing, melting and water quenching to obtain NZSP glass;
[0027] b) mixing the Na source compound, the Zr source compound, the Si source compound, the P source compound and the NZSP glass, ball milling, calcining, crushing, pressing and sintering to obtain a modified NASICON type sodium ion solid electrolyte.
[0028] In the method provided by the present invention, in step a), the Na source compound is preferably Na2CO3; the Zr source compound is preferably ZrO2; the Si source compound is preferably SiO2; and the P source compound is preferably NH4H2PO4.
[0029] In the method provided by the present invention, in step a), based on the molar amounts of Na, Zr, Si and P, the molar ratio of the Na source compound, the Zr source compound, the Si source compound and the P source compound is (47-52):(11-14):(50-55):10, preferably 49:13.5:52:10.
[0030] In the method provided by the present invention, in step a), the ball milling method is preferably wet milling; the liquid medium used in the wet milling is preferably ethanol; the rotation speed of the wet milling is preferably 400-800 r / min, specifically 400 r / min, 450 r / min, 500 r / min, 550 r / min, 600 r / min, 650 r / min, 700 r / min, 750 r / min or 800 r / min; the wet milling time is preferably 4-8 h, specifically 4 h, 4.5 h, 5 h, 5.5 h, 6 h, 6.5 h, 7 h, 7.5 h or 8 h; after the wet milling is completed, drying is required to remove the liquid phase in the wet milled slurry, and the drying temperature is preferably 75-150 ° C.
[0031] In the method provided by the present invention, in step a), impurities and volatile substances in the mixture are removed by calcination; the calcination is carried out in an aerobic environment, and the aerobic environment is preferably an air atmosphere; the calcination temperature is preferably 750-1050°C, specifically 750°C, 800°C, 850°C, 900°C, 950°C, 1000°C or 1050°C; the calcination time is preferably 2-6h, specifically 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, 5h, 5.5h or 6h.
[0032] In the method provided by the present invention, in step a), the pulverization method is preferably: first crushing into large pieces, and then ball milling into fine powder. Wherein, the ball milling method is preferably wet milling; the liquid medium used in the wet milling is preferably ethanol; the rotation speed of the wet milling is preferably 400-800r / min, specifically 400r / min, 450r / min, 500r / min, 550r / min, 600r / min, 650r / min, 700r / min, 750r / min or 800r / min; the wet milling time is preferably 4-8h, specifically 4h, 4.5h, 5h, 5.5h, 6h, 6.5h, 7h, 7.5h or 8h; after the wet milling is completed, it is necessary to dry to remove the liquid phase in the wet milled slurry, and the drying temperature is preferably 75-150°C.
[0033] In the method provided by the present invention, in step a), the melting temperature is preferably 1300-1550°C, specifically 1300°C, 1350°C, 1400°C, 1450°C, 1500°C or 1550°C; the melting time is preferably 2.5-5h, specifically 2.5h, 3h, 3.5h, 4h, 4.5h or 5h.
[0034] In the method provided by the present invention, in step a), after the water quenching is completed, slag-like NZSP glass is obtained. For the convenience of subsequent use, the slag-like NZSP glass is preferably further ground into powder.
[0035] In the method provided by the present invention, in step b), the Na source compound is preferably Na2CO3; the Zr source compound is preferably ZrO2; the Si source compound is preferably SiO2; and the P source compound is preferably NH4H2PO4.
[0036] In the method provided by the present invention, in step b), the chemical formula Na 1+x Zr2Si x P 3-x O 12 (0<x<3) is used as a reference to calculate the raw material ratio of the required Na source compound, Zr source compound, Si source compound and P source compound. Preferably, based on the molar amount of Na, Zr, Si and P, the molar ratio of the Na source compound, Zr source compound, Si source compound and P source compound is (2.5~3.5):2:(1.5~2.5):(0.5~1.5), more preferably 3:2:2:1.
[0037] In the method provided by the present invention, in step b), the NZSP glass preferably accounts for 1-10% of the total mass of the Na source compound, the Zr source compound, the Si source compound, the P source compound and the NZSP glass, and specifically may be 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9% or 10%.
[0038] In the method provided by the present invention, in step b), the ball milling method is preferably wet milling; the liquid medium used in the wet milling is preferably ethanol; the rotation speed of the wet milling is preferably 400-800 r / min, specifically 400 r / min, 450 r / min, 500 r / min, 550 r / min, 600 r / min, 650 r / min, 700 r / min, 750 r / min or 800 r / min; the wet milling time is preferably 4-8 h, specifically 4 h, 4.5 h, 5 h, 5.5 h, 6 h, 6.5 h, 7 h, 7.5 h or 8 h; after the wet milling is completed, drying is required to remove the liquid phase in the wet milled slurry, and the drying temperature is preferably 75-150 ° C.
[0039] In the method provided by the present invention, in step b), impurities and volatile substances in the mixture are removed by calcination; the calcination is carried out in an aerobic environment, and the aerobic environment is preferably an air atmosphere; the calcination temperature is preferably 750-1050°C, specifically 750°C, 800°C, 850°C, 900°C, 950°C, 1000°C or 1050°C; the calcination time is preferably 2-6h, specifically 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, 5h, 5.5h or 6h.
[0040] In the method provided by the present invention, in step b), the pulverization method is preferably: first crushing into large pieces, and then ball milling into fine powder. Wherein, the ball milling method is preferably wet milling; the liquid medium used in the wet milling is preferably ethanol; the rotation speed of the wet milling is preferably 400-800r / min, specifically 400r / min, 450r / min, 500r / min, 550r / min, 600r / min, 650r / min, 700r / min, 750r / min or 800r / min; the wet milling time is preferably 4-8h, specifically 4h, 4.5h, 5h, 5.5h, 6h, 6.5h, 7h, 7.5h or 8h; after the wet milling is completed, it is necessary to dry to remove the liquid phase in the wet milled slurry, and the drying temperature is preferably 75-150°C.
[0041] In the method provided by the present invention, in step b), the pressing pressure is preferably 4-8 MPa, specifically 4 MPa, 4.5 MPa, 5 MPa, 5.5 MPa, 6 MPa, 6.5 MPa, 7 MPa, 7.5 MPa or 8 MPa; the material obtained by pressing is a sheet, and the thickness of the sheet is preferably 1-2 mm, specifically 1.2 mm.
[0042] In the method provided by the present invention, in step b), the sintering is carried out in an aerobic environment, and the aerobic environment is preferably an air atmosphere; the sintering temperature is preferably 1000-1300°C, and can be specifically 1000°C, 1050°C, 1080°C, 1100°C, 1150°C, 1200°C, 1250°C or 1300°C; the sintering time is preferably 6-10h, and can be specifically 6h, 6.5h, 7h, 7.5h, 8h, 8.5h, 9h, 9.5h or 10h.
[0043] The method provided by the present invention can prepare NASICON-type oxide solid electrolyte materials with excellent performance under low sintering temperature conditions. More specifically, the method has the following beneficial effects:
[0044] (1) The present invention adjusts the raw material ratio of the initial sodium source, silicon source, zirconium source, and phosphorus source, mixes them, melts them, and then quenches them with water to form a clear, transparent, impurity-free NZSP glass. The NZSP glass has a relatively low melting temperature (800-950°C). In the process of sintering to prepare the NASICON type sodium ion solid electrolyte, the NZSP glass is added as a sintering aid. During the sintering process, the NZSP glass becomes a liquid phase with fluidity, can wet the powder raw materials, promote material migration, enable the grains to grow rapidly, and fill the pores between the grain boundaries, thereby improving the density of the sintered product and reducing the sintering temperature and time.
[0045] (2) Sintering is also a heat treatment process for NZSP glass. The ZrO2 impurity phase produced by sintering can be reacted during the crystallization process of the grain boundary glass. Most of the ZrO2 impurity phase can be removed while the sodium zirconium phosphate conductive crystal phase is precipitated in the NZSP glass. This NZSP microcrystalline glass has a certain ionic conductivity. The NZSP microcrystalline glass at the grain boundary after heat treatment provides a path for sodium ion migration, which alleviates the grain boundary interface impedance.
[0046] (3) NZSP glass with the same components is used as a sintering aid in the sintering process. Without the introduction of other elements, the ionic conductivity of the grain boundaries is improved. At the same time, it also has the function of replenishing sodium for the grain body. It is only necessary to control the composition of the original glass components and the final sintering temperature to complete the preparation of NASICON-type oxide solid electrolytes with high density, high ionic conductivity and low impurity content.
[0047] For the purpose of greater clarity, the present invention is described in detail with reference to the following examples and comparative examples.
[0048] Example 1
[0049] (1) Using Na2CO3, ZrO2, SiO2, and NH4H2PO4 as glass components, multiple melting-water quenching tests were carried out on mixed powders with different raw material ratios. The raw material ratio design is shown in Table 1:
[0050] Table 1
[0051]
[0052] The specific experimental process and experimental results are as follows:
[0053] According to the proportions in Table 1, the four raw materials were mixed in a corundum ball mill with anhydrous ethanol, ball milled at a speed of 600r / min for 8h on a planetary ball mill, and then dried in a blast drying oven at 80°C overnight; the dried powder was calcined in a muffle furnace at a temperature of 800°C for 3h to remove impurities and volatile substances, the calcination atmosphere was air, and the lumps were manually broken after calcination, and further ball milled with anhydrous ethanol (600r / min) for 6h, and the slurry after ball milling was dried in a blast drying oven at 80°C overnight; the dried powder was placed in an arc-shaped alumina crucible and placed in a lifting glass melting furnace to fully melt, and kept at 1450°C for 3h to fully melt the raw material powder, and then the molten liquid was quickly taken out and poured into an iron bucket filled with deionized water for water quenching, and the quenched glass slag was dried in a blast drying oven at 80°C overnight to remove excess moisture, and was manually crushed into coarse glass powder in an agate mortar.
[0054] The preparation of glass powder under different raw material ratios was evaluated. The results showed that when the molar mass ratio of the four raw materials Na2CO3, ZrO2, SiO2, and NH4H2PO4 was 24.5:13.5:52:10, a clear, transparent, impurity-free NZSP glass with a sodium zirconium phosphate conductive crystal phase precipitated after sintering could be successfully obtained. The melting temperature of the NZSP glass was 800-950°C. When the raw materials were in other molar mass ratios, at least one of the following problems would occur:
[0055] ①The raw materials cannot be fully melted;
[0056] ②After the raw material is melted, the viscosity is too high and it cannot be poured out of the crucible;
[0057] ③ Too much raw material is lost during the melting process;
[0058] ④ The raw material is not clear and transparent after melting, and the inside is turbid and fragile after cooling;
[0059] ⑤ Even if glass in good condition is obtained, it is difficult to obtain a conductive crystal phase after sintering.
[0060] (2) The four raw materials with the best ratio (the molar mass ratio of Na2CO3, ZrO2, SiO2, and NH4H2PO4 is 24.5:13.5:52:10) are mixed with anhydrous ethanol in a corundum ball mill, and ball milled at a speed of 600 r / min for 8 h on a planetary ball mill, and then dried in a forced air drying oven at 80°C overnight; the dried powder is calcined in a muffle furnace at 800°C for 3 h to remove impurities and volatile substances in an air calcination atmosphere. After calcination, the agglomerates are manually broken and further The mixture was ball-milled with anhydrous ethanol (600 r / min) for 6 h, and the slurry after ball milling was dried in a forced air drying oven at 80°C overnight; the dried powder was placed in an arc-shaped alumina crucible and placed in a lifting glass melting furnace to fully melt, and kept warm at 1450°C for 3 h to fully melt the raw material powder, and then the clear and transparent liquid was quickly taken out and poured into an iron bucket filled with deionized water for water quenching, and the glass slag after water quenching was dried in a forced air drying oven at 80°C overnight to remove excess moisture, and manually crushed into coarse glass powder (powder A) in an agate mortar for later use.
[0061] (3) With the chemical formula Na3Zr2Si2PO 12 The four raw materials of Na2CO3, ZrO2, SiO2 and NH4H2PO4 were prepared as the basis, that is, the molar mass ratio of the four raw materials of Na2CO3, ZrO2, SiO2 and NH4H2PO4 was 1.5:2:2:1, and the mixed powder was recorded as powder B; powder B and the powder A prepared above were mixed in anhydrous ethanol at a mass ratio of 97:3 in a corundum ball mill, and a series of operations such as ball milling, calcination, crushing and drying were carried out according to the steps and conditions for preparing powder A in (2) (without melting and water quenching) to obtain powder C; powder C was cold-pressed into a disc with a diameter of 1.6 cm and a thickness of 1.2 mm under a hydraulic press at a pressure of 6 MPa; the disc was placed on an alumina plate and sintered in a muffle furnace in an air atmosphere at a temperature of 1050°C for 5 h to obtain a final modified solid electrolyte.
[0062] Example 2
[0063] Referring to Example 1, the only difference is that the mass ratio of powder A to powder B is 5:95, and the final modified solid electrolyte is obtained.
[0064] Example 3
[0065] Referring to Example 1, the only difference is that the mass ratio of powder A to powder B is 7:93, and the final modified solid electrolyte is obtained.
[0066] Example 4
[0067] Referring to Example 1, the only difference is that the mass ratio of powder A to powder B is 9:91, and the final modified solid electrolyte is obtained.
[0068] Example 5
[0069] Refer to Example 1, the only difference is that the sintering temperature is 1080° C. to obtain the final modified solid electrolyte.
[0070] Example 6
[0071] Refer to Example 1, the only difference is that the sintering temperature is 1150° C. to obtain the final modified solid electrolyte.
[0072] Comparative Example 1
[0073] Referring to Example 1, the only difference is that powder A is not added to obtain a solid electrolyte.
[0074] Comparative Example 2
[0075] Referring to Example 1, the only difference is that powder A is not added, the sintering temperature is 1250° C., and a solid electrolyte is obtained.
[0076] Performance testing and evaluation
[0077] The solid electrolytes obtained in Examples 1 to 6 and Comparative Examples 1 to 2 were tested for ionic conductivity, relative density and Zr2O impurity content.
[0078] (1) Test of ionic conductivity:
[0079] The two sides of the electrolyte sheet were polished and polished with 400 mesh, 2000 mesh, and 5000 mesh sandpaper to remove surface impurities and smoothen them to ensure uniform thickness and surface. After polishing, they were ultrasonically cleaned with anhydrous ethanol for 30 minutes and dried in a 60°C forced air drying oven for 2 hours. Then, an ion sputtering instrument was used to spray gold on both sides of the electrolyte sheet as ion blocking electrodes. Before testing, the gold on the side of the electrolyte sheet was polished off with sandpaper, and its thickness D and cross-sectional area S were measured with a vernier caliper. Its AC impedance R was measured, and the ionic conductivity (S / cm) was calculated according to the formula σ=D / SR.
[0080] (2) Relative density test:
[0081] Continue to dry the sample and weigh it every two hours. When the difference between two adjacent masses does not exceed 0.5%, the weight at this time can be considered as the dry mass of the sample m1. Boil the sample in distilled water for 3 hours to ensure sufficient water absorption. Then put the sample in a hanging basket and immerse it in the liquid to measure its mass to obtain m21. Take out the sample and measure the weight of the hanging basket at the same position m22. Subtract m22 from m21 to obtain the floating weight m2. Take out the wet sample, gently wipe off the surface moisture, and weigh it to obtain the mass of the wet sample m3. Use the formula ρ = ρ1 × m1 / (m3-m2) to calculate the density, where ρ is the volume density (g / cm3 );ρ1 is the density of the immersed liquid at the experimental temperature (g / cm 3 ), here we take 0.997g / cm3; m1 is the mass of dry sample (g); m3 is the mass of wet sample (g); m2 is the floating weight (g). The measured density compared with the theoretical density is the relative density of the sample.
[0082] (3) Test of Zr2O impurity content:
[0083] The crystal structure Na3Zr2Si2PO 12 (CSD:202154) is the basic model ( α=90°, β=123.742°, γ=90°, ), and the X-ray diffraction data were refined by Rietveld full spectrum fitting using the FullProf program to obtain the Zr2O impurity content.
[0084] Test data see Table 2
[0085] Table 2
[0086] Sintering temperature(℃) Ionic conductivity (S / cm) Relative density (%) <![CDATA[ZrO2 content (wt%)]]> Example 1 1050 <![CDATA[4.7×10 -4 ]]> 91.5 6.4 Example 2 1050 <![CDATA[7.8×10 -4 ]]> 94.2 3.8 Example 3 1050 <![CDATA[8.9×10 -4 ]]> 97.9 1.3 Example 4 1050 <![CDATA[8.5×10 -4 ]]> 96.9 1.7 Example 5 1080 <![CDATA[9.1×10 -4 ]]> 97.7 1.7 Example 6 1150 <![CDATA[7.9×10 -4 ]]> 96.1 1.8 Comparative Example 1 1050 <![CDATA[9.3×10 -5 ]]> 81.7 11.2 Comparative Example 2 1250 <![CDATA[3.2×10 -4 ]]> 89.9 7.9
[0087] By comparing Examples 1 to 6 with Comparative Example 1, it can be seen that at the same sintering temperature, the samples doped with glass exhibited higher ionic conductivity and relative density. The addition of glass effectively promoted material transfer and reaction, and NZSP solid electrolytes with higher ionic conductivity were prepared at a temperature lower than the conventional solid phase reaction temperature. When no glass was added, the densification sintering of the NZSP solid electrolyte could not be completed at a temperature of 1050°C, the reaction activity between the substances was low, there were many impurities, the material was porous inside, and the sodium ion transmission was hindered (see Figure 1-2 In addition, as the amount of glass increases, the ionic conductivity of the samples of Examples 1 to 4 shows a trend of first increasing and then decreasing. This is because the addition of appropriate glass alleviates the grain boundary resistance, and the sodium zirconium phosphate conductive phase after crystallization promotes the transmission of sodium ions at the grain boundaries. When the content of NZSP glass is too high, it will flow through the grains between crystals, leaving submicron-sized pores (see Figure 2-3), such small holes will hinder the migration of sodium ions and reduce the relative density of the sample. From Examples 5 and 6, when the mass ratio of NZSP glass powder to ceramic powder is 7:93, a NZSP solid electrolyte with high density, low ZrO2 impurity content and high ionic conductivity can be obtained within the range of 1050-1100°C. When the sample contains glass, excessively high temperature (1150°C) will also aggravate the flow of glass, thereby leaving submicron-sized small holes inside the grains to hinder the transmission of sodium ions. By comparing Examples 1-6 with Comparative Example 2, it can be seen that sintering the NZSP solid electrolyte at a high temperature of 1250°C will increase the relative density of the sample to a certain extent, thereby improving the ionic conductivity, but the volatilization of light elements at high temperature will cause the formation of impurity ZrO2. It can be seen from Table 2 that the ZrO2 impurity of the sample in Comparative Example 2 is increased relative to that in the embodiment, which is obviously not conducive to the internal ion transmission of the NZSP electrolyte.
[0088] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a modified NASICON type sodium ion solid electrolyte, It is characterized in that The following steps are involved: a) mixing a Na source compound, a Zr source compound, a Si source compound and a P source compound, ball milling, calcining, crushing, melting and water quenching to obtain NZSP glass; In step a), based on the molar amounts of Na, Zr, Si and P, the molar ratio of the Na source compound, the Zr source compound, the Si source compound and the P source compound is (47-52):(11-14):(50-55):10; b) mixing the Na source compound, the Zr source compound, the Si source compound, the P source compound and the NZSP glass, ball milling, calcining, crushing, pressing and sintering to obtain a modified NASICON type sodium ion solid electrolyte.
2. The method according to claim 1, It is characterized in that In step a), based on the molar amounts of Na, Zr, Si and P, the molar ratio of the Na source compound, the Zr source compound, the Si source compound and the P source compound is 49:13.5:52:
10.
3. The method according to claim 1, It is characterized in that In step a), the Na source compound is Na 2 CO 3 ; The Zr source compound is ZrO 2 ; The Si source compound is SiO 2 ; The P source compound is NH 4 H 2 PO 4 .
4. The method according to claim 1, It is characterized in that In step a), the calcination temperature is 750-1050° C. and the calcination time is 2-6 hours.
5. The method according to claim 1, It is characterized in that In step a), the melting temperature is 1300-1550° C.; the melting time is 2.5-5 hours.
6. The method according to claim 1, It is characterized in that In step b), the Na source compound is Na 2 CO 3 ; The Zr source compound is ZrO 2 ; The Si source compound is SiO 2 ; The P source compound is NH 4 H 2 PO 4 .
7. The method according to claim 1, It is characterized in that In step b), based on the molar amounts of Na, Zr, Si and P, the molar ratio of the Na source compound, Zr source compound, Si source compound and P source compound is (2.5-3.5):2:(1.5-2.5):(0.5-1.5).
8. The method according to claim 1, It is characterized in that In step b), the NZSP glass accounts for 1-10% of the total mass of the Na source compound, the Zr source compound, the Si source compound, the P source compound and the NZSP glass.
9. The method according to claim 1, It is characterized in that In step b), the calcination temperature is 750-1050° C. and the calcination time is 2-6 hours.
10. The method according to claim 1, It is characterized in that In step b), the sintering temperature is 1000-1300° C. and the sintering time is 6-10 hours.