Novel composite polymer-based solid electrolyte as well as preparation method and application thereof
Synthesis of fluorine-containing metal organic frame MOF fillers by hydrothermal method, reducing the crystallinity of PEO-based solid electrolytes, solving the problems of unfavorable lithium ion conduction and unstable interface at room temperature, and improving the ionic conductivity and cycling performance of the battery .
Patent Information
- Application Number
- CN202410197636.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-22
- Publication Date
- 2024-11-22
AI Technical Summary
The traditional polyethylene oxide (PEO)-based solid electrolyte has a high crystallinity at room temperature, resulting in unfavorable conduction of lithium ions and an unstable interface with lithium metal, affecting the battery's ultra-long cycle life.
The hydrothermal method is used to synthesize fluorine-containing metal organic frame MOF as a filler to reduce the crystallinity of PEO, and stir evenly with the lithium salt and the polymer substrate, cast and mold to form a composite polymer-based solid electrolyte, and promote the interface formation of lithium conduction properties.
The ionic conductivity of the electrolyte and the long cycle performance of the battery are improved, and a stable negative electrode/electrolyte interface is formed, and the uniform deposition of Li+ is adjusted, which improves the cycle stability of the battery.
Smart Images

Figure CN119009090A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of solid-state battery materials, and in particular relates to a novel composite polymer-based solid-state electrolyte and a preparation method and application thereof. Background Art
[0002] With the development of the times, society has higher and higher requirements for energy storage devices. Due to the advantages of high operating voltage, long cycle life and low environmental pollution, lithium batteries have been widely used in high-end fields such as consumer electronics, electric vehicles and even aerospace. However, traditional liquid lithium batteries have a series of safety problems such as easy leakage and extremely easy to catch fire due to the use of organic electrolytes. Using solid electrolytes instead of traditional liquid organic electrolytes is an effective way to improve battery safety performance. Traditional solid electrolytes are divided into sulfide solid electrolytes, oxide solid electrolytes, halide solid electrolytes, polymer solid electrolytes, etc. However, at this point in time, it is still challenging to manufacture large-scale inorganic all-solid electrolytes (SIEs) such as oxides and sulfides, and the cost is too high to be practical. Compared with inorganic solid electrolytes, polymer solid electrolytes (SPEs) have higher flexibility, better processing performance and better compatibility with lithium. Taking the most mature polyethylene oxide (PEO)-based solid electrolyte as an example, it has strong lithium salt dissociation ability, low price and easy processing. However, its high crystallinity at room temperature is not conducive to the conduction of lithium ions, and the unstable interface formed between it and lithium metal is not conducive to the ultra-long cycle life of the battery. Studies have shown that nanoparticles with Lewis acidic surface properties are of special significance for improving ion conductivity. These highly designable nanofillers have abundant polar groups, which can promote the dissociation of lithium salts through Lewis acid-base interactions and enhance ion transport capacity. Composite polymer-based solid electrolytes prepared with them as fillers in polymer solid electrolytes are more conducive to forming a stable negative electrode / electrolyte interface and regulating Li + The uniform deposition of the electrolyte improves the long cycle performance of the battery. In particular, some porous fillers grafted with organic functional groups, such as MOF and COF, have hybrid properties, which improve the miscibility with PEO, thereby improving the ionic conductivity and stability of the electrolyte. Summary of the invention
[0003] The purpose of the present invention is to solve the problem that the PEO ion conductivity is low and the interface formed between the PEO and the lithium metal is unstable, and to provide a novel composite polymer-based solid electrolyte and a preparation method and application thereof.
[0004] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0005] A method for preparing a novel composite polymer-based solid electrolyte, the method comprising:
[0006] Step 1: dissolving a certain amount of zinc ion salt in a polar solvent to obtain solution A, and stirring evenly;
[0007] Step 2: dissolving the organic ligand in a polar solvent to obtain solution B, and stirring evenly;
[0008] Step 3: Slowly introduce solution A into solution B and stir evenly for 1 hour, then transfer to a reactor for hydrothermal reaction;
[0009] Step 4: After the reaction time is up, the obtained solution is centrifuged to obtain the bottom particles and vacuum dry them to obtain white particles;
[0010] Step 5: The white particles are removed by a Soxhlet extractor, and then the removed particles are placed in a vacuum drying oven to be fully dried to obtain a metal organic framework MOF;
[0011] Step 6: dissolving the lithium salt, metal organic framework MOF and polymer substrate in a polar solvent in sequence and stirring evenly to obtain a homogeneous solution;
[0012] Step 7: pouring the obtained uniform solution into a mold containing flexible fibers to form it uniformly;
[0013] Step 8: Transfer the mold to an inert gas-protected glove box for drying and removing the organic solution; transfer the formed electrolyte membrane to a vacuum drying oven for thorough drying to obtain a new composite polymer-based solid electrolyte.
[0014] Furthermore, in step 1, the zinc ion salt is one of zinc acetate, zinc sulfate, and zinc nitrite, with a mass of 0.2 to 0.4 g, and the polar solvent is one of methanol and N-methylformamide; in step 2, the organic ligand is one of fluorine-containing imidazoles such as 4-fluoro-1H-imidazole and 4(5)-(trifluoromethyl)imidazole.
[0015] Furthermore, in step three, the molar ratio of the organic ligand to the zinc ion salt is 1:2-4; the hydrothermal temperature is 120-160° C., and the time is 24-36 hours.
[0016] Furthermore, in step 4, the drying temperature is 60° C. and the drying time is 12 h.
[0017] Furthermore, in step five, the Soxhlet extractor is used for impurity removal for 24 hours, the vacuum drying temperature is 100° C., and the drying time is 12 hours.
[0018] Furthermore, in step six, the lithium salt is one of LiTFSI, LiClO4, and LiFSI, the polymer substrate is one of polyethylene oxide (PEO), polytetrafluoroethylene (PVDF), and polymethyl methacrylate (PMMA), and the polar solvent is acetonitrile or dimethyl sulfoxide; in the homogeneous solution, the molar ratio of the lithium salt to the polymer substrate is 1:10, and the mass ratio of the metal organic framework MOF to the polymer substrate is 1 to 2:10 (preferably 1:10, 1.5:10, 2:10), and the role of the polar solvent is to dissolve the above solutes.
[0019] Furthermore, in step seven, the flexible fiber is one of non-woven fabric, polyacrylonitrile carbon nanofiber, and PI fiber.
[0020] Furthermore, in step eight, the drying time of the solution in the glove box is 12 hours, and the drying temperature is 60-80° C.; the drying temperature of the vacuum drying oven is 60° C., and the drying time is 10-15 hours.
[0021] A novel composite polymer-based solid electrolyte prepared by the above preparation method.
[0022] A novel composite polymer-based solid electrolyte prepared by the above preparation method is used in the preparation of a composite polymer-based solid-state battery, wherein the composite polymer-based solid-state battery is assembled from materials including a lithium negative electrode, a composite polymer-based solid-state electrolyte material, and a positive electrode material; the positive electrode material is one of high-voltage positive electrode materials such as LiFePO4, LiCoO2, and NCM811.
[0023] The present invention utilizes a hydrothermal method to prepare and synthesize a novel fluorine-containing metal organic framework MOF, and successively dissolves it with a lithium salt and a polymer substrate in a polar solvent and stirs them uniformly. After obtaining a homogeneous solution, it is poured into a mold containing a non-woven fabric and uniformly formed. After a series of drying processes, a novel composite polymer-based solid electrolyte is obtained.
[0024] The beneficial effects of the present invention compared with the prior art are as follows: the use of a hydrothermal method to synthesize a new MOF and use it in the preparation of a composite polymer solid electrolyte is a preparation method with a simple process, easy operation, and suitable for industrial production of a new composite polymer-based solid electrolyte.
[0025] The present invention prepares a new type of fluorinated metal organic framework MOF as a filler for PEO-based polymer solid electrolyte, which effectively breaks the crystallinity of PEO and improves the ionic conductivity. At the same time, it helps to catalyze the formation of an artificial SEI layer with lithium conductive properties at the negative electrode interface, which can regulate Li + The uniform deposition of MOF fillers helps to improve the stability of the electrolyte / lithium negative electrode interface. The polymer solid-state battery modified with MOF fillers exhibits excellent long-cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a SEM image of the metal organic framework MOF prepared in Example 1;
[0027] Figure 2 The first charge and discharge curve of the composite polymer solid-state battery prepared in Example 1 at a current density of 0.5C and a voltage range of 2.5 to 4.1V;
[0028] Figure 3 The cycle performance diagram of the composite polymer solid-state battery prepared in Example 1 at a current density of 0.5C and a voltage range of 2.5 to 4.1V;
[0029] Figure 4 This is a SEM image of the metal organic framework MOF prepared in Example 4;
[0030] Figure 5 The first charge and discharge curve of the polymer solid-state battery prepared in the comparative example at 0.5C current density and 2.5-4.1V voltage range;
[0031] Figure 6 It is a cycle performance diagram of the first charge and discharge curve of the polymer solid-state battery prepared in the comparative example at a current density of 0.5C and a voltage range of 2.5 to 4.1V;
[0032] Figure 7 It is a comparison chart of the cycle performance of Example 1 and the comparative example. DETAILED DESCRIPTION
[0033] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and embodiments, but is not limited thereto. Any modification or equivalent replacement of the technical solution of the present invention that does not depart from the spirit and scope of the technical solution of the present invention should be included in the protection scope of the present invention.
[0034] The present invention uses a hydrothermal method to prepare a metal organic framework MOF containing poly-F ligands, and uses it as a filler for pure polymer solid electrolytes, thereby reducing the crystallinity of PEO solid electrolytes and improving the ionic conductivity of electrolyte membranes. At the same time, during the battery cycle, the formation of a stable lithium metal / electrolyte interface is promoted, and the long cycle performance of PEO-based solid-state batteries is improved, which has potential application prospects.
[0035] Example 1
[0036] A method for preparing a novel composite polymer comprises the following steps:
[0037] 0.1g zinc acetate was dissolved in methanol to obtain solution A, which was stirred evenly; 0.4g 4(5)-(trifluoromethyl)imidazole was dissolved in methanol to obtain solution B, which was stirred evenly; solution A was slowly introduced into solution B and stirred evenly for 1 hour, then transferred to a reactor and hydrothermally reacted at 120°C for 24 hours. After the reaction time was up, the obtained solution was centrifuged to obtain the bottom particles and vacuum dried at 60°C, and white particles were obtained after 12 hours. The white particles were removed by Soxhlet extractor, and then the removed particles were placed in a vacuum drying oven at 100°C for 12 hours. After sufficient drying, a new type of metal organic framework MOF was obtained, labeled as ZIFs-F; LiTFSI, ZIFs-F and PEO substrate (M LiTFS :M PEO =1:10, m ZIFs-F :m PEO =1:10) are successively dissolved in acetonitrile and stirred uniformly to obtain a homogeneous solution; the obtained uniform solution is poured into a mold containing a non-woven fabric to make it uniformly formed; the mold is transferred to a glove box protected by an inert gas, dried at 60°C for 12 hours, and the acetonitrile is removed; the formed electrolyte membrane is transferred to a vacuum drying oven, dried at 60°C for 12 hours, and a new type of composite polymer-based solid electrolyte is obtained, which is marked as PEO-10% ZIFs-3F.
[0038] The PEO-10% ZIFs-F composite polymer solid electrolyte prepared in this embodiment is used as the electrolyte material of the composite polymer solid-state battery. The composite polymer-based solid-state battery is assembled from materials including a lithium negative electrode, a composite polymer solid electrolyte material, and a positive electrode material; the positive electrode material is one of the high-voltage positive electrode materials such as LiFePO4, LiCoO4, and NCM811, and a button cell is assembled for electrochemical performance testing. The test conditions are that the charge and discharge cut-off voltage is 2.5-4.1V, and the test current is 0.1C (1C = 170mAh g -1 ).
[0039] The SEM image of the metal organic framework MOF prepared in this example is as follows Figure 1 As shown, observe Figure 1 It can be seen that the prepared MOF particles have a spherical structure with a particle size of about 10 μm.
[0040] According to the ionic conductivity formula: ionic conductivity L is the electrolyte thickness, R is the impedance, and S is the electrolyte area. The ionic conductivity of the composite polymer solid electrolyte at room temperature is calculated to be 4.27×10 -5 S cm -1 .
[0041] The composite polymer solid electrolyte material prepared in this embodiment is used in a polymer solid-state battery. The first charge and discharge curve under 0.5C and 2.5-4.1V is as follows: Figure 2 As shown. Figure 2 It can be seen that its first discharge capacity is 152mAh g -1 , the first coulombic efficiency is 97.2%.
[0042] The composite polymer solid electrolyte material prepared in this embodiment is used in polymer solid-state batteries. The cycle performance under 0.5C and 2.5-4.1V conditions is shown in the figure below: Figure 3 As shown. Figure 3 It can be seen that the material exhibits good cycle stability.
[0043] Example 2
[0044] A method for preparing a novel composite polymer comprises the following steps:
[0045] 0.1g zinc acetate was dissolved in methanol to obtain solution A, which was stirred evenly; 0.4g 4(5)-(trifluoromethyl)imidazole was dissolved in methanol to obtain solution B, which was stirred evenly; solution A was slowly introduced into solution B and stirred evenly for 1 hour, then transferred to a reactor and hydrothermally reacted at 120°C for 24 hours. After the reaction time was up, the obtained solution was centrifuged, the bottom particles were obtained and vacuum dried at 60°C, and white particles were obtained after 12 hours. The white particles were removed by Soxhlet extractor, and then the removed particles were placed in a vacuum drying oven at 100°C for 12 hours. After sufficient drying, a new type of metal organic framework MOF was obtained, labeled as ZIFs-F; LiTFSI, ZIFs-F and PEO substrate (M LiTFS :M PEO =1:10, m ZIFs-F :m PEO =1.5:10) are successively dissolved in acetonitrile and stirred uniformly to obtain a homogeneous solution; the obtained uniform solution is poured into a mold containing a non-woven fabric to make it uniformly formed; the mold is transferred to a glove box protected by an inert gas, dried at 60°C for 12 hours, and the acetonitrile is removed; the formed electrolyte membrane is transferred to a vacuum drying oven, dried at 60°C for 12 hours, and a new type of composite polymer-based solid electrolyte is obtained, which is marked as PEO-15% ZIFs-3F.
[0046] The positive electrode material matched in this embodiment is the same as that in embodiment 1. The test conditions are as follows: the charge and discharge cut-off voltage is 2.5-4.1V, and the test current is 0.1C (1C = 170mAh g -1 ).
[0047] According to the ionic conductivity formula: ionic conductivity L is the electrolyte thickness, R is the impedance, and S is the electrolyte area. The ionic conductivity of the composite polymer solid electrolyte at room temperature is calculated to be 3.83×10 -5 S cm -1 .
[0048] Example 3
[0049] A method for preparing a novel composite polymer comprises the following steps:
[0050] 0.1g zinc acetate was dissolved in methanol to obtain solution A, which was stirred evenly; 0.4g 4(5)-(trifluoromethyl)imidazole was dissolved in methanol to obtain solution B, which was stirred evenly; solution A was slowly introduced into solution B and stirred evenly for 1 hour, then transferred to a reactor and hydrothermally reacted at 120°C for 24 hours. After the reaction time was up, the obtained solution was centrifuged to obtain the bottom particles and vacuum dried at 60°C, and white particles were obtained after 12 hours. The white particles were removed by Soxhlet extractor, and then the removed particles were placed in a vacuum drying oven at 100°C for 12 hours. After sufficient drying, a new type of metal organic framework MOF was obtained, labeled as ZIFs-F; LiTFSI, ZIFs-F and PEO substrate (M LiTFS :M PEO =1:10, m ZIFs-F :m PEO =1:20) are successively dissolved in acetonitrile and stirred uniformly to obtain a homogeneous solution; the obtained uniform solution is poured into a mold containing a non-woven fabric to make it uniformly formed; the mold is transferred to a glove box protected by an inert gas, dried at 60°C for 12 hours, and the acetonitrile is removed; the formed electrolyte membrane is transferred to a vacuum drying oven, dried at 60°C for 12 hours, and a new type of composite polymer-based solid electrolyte is obtained, which is marked as PEO-5%ZIFs-3F.
[0051] The composite polymer solid electrolyte matched in this embodiment is the same as that in embodiment 1. The test conditions are as follows: the charge and discharge cut-off voltage is 2.5-4.1V, the test current is 0.1C (1C = 170mAh g -1 ).
[0052] The positive electrode material matched in this embodiment is the same as that in embodiment 1. The test conditions are as follows: the charge and discharge cut-off voltage is 2.5-4.1V, and the test current is 0.1C (1C = 170mAh g -1 ).
[0053] According to the ionic conductivity formula: ionic conductivity L is the electrolyte thickness, R is the impedance, and S is the electrolyte area. The ionic conductivity of the composite polymer solid electrolyte at room temperature is calculated to be 3.65×10 -5 S cm -1 .
[0054] Example 4
[0055] A method for preparing a novel composite polymer comprises the following steps:
[0056] 0.1g zinc acetate was dissolved in methanol to obtain solution A, which was stirred evenly; 0.4g 4-fluoro-1H-imidazole was dissolved in methanol to obtain solution B, which was stirred evenly; solution A was slowly introduced into solution B and stirred evenly for 1 hour, then transferred to a reactor and hydrothermally reacted at 120°C for 24 hours. After the reaction time was up, the obtained solution was centrifuged to obtain the bottom particles and vacuum dried at 60°C, and white particles were obtained after 12 hours. The white particles were removed by Soxhlet extractor, and then the removed particles were placed in a vacuum drying oven at 100°C for 12 hours. After sufficient drying, a new type of metal organic framework MOF was obtained, labeled as ZIFs-F; LiTFSI, ZIFs-F and PEO substrate (M LiTFS :M PEO =1:10, m ZIFs-F :m PEO =1:10) are successively dissolved in acetonitrile and stirred uniformly to obtain a homogeneous solution; the obtained uniform solution is poured into a mold containing a non-woven fabric to make it uniformly formed; the mold is transferred to a glove box protected by an inert gas, dried at 60°C for 12 hours, and the acetonitrile is removed; the formed electrolyte membrane is transferred to a vacuum drying oven, dried at 60°C for 12 hours, and a new type of composite polymer-based solid electrolyte is obtained, which is marked as PEO-10% ZIFs-F.
[0057] The composite polymer solid electrolyte matched in this embodiment is the same as that in embodiment 1. The test conditions are as follows: the charge and discharge cut-off voltage is 2.5-4.1V, the test current is 0.1C (1C = 170mAh g -1 ).
[0058] The SEM image of the metal organic framework MOF prepared in the embodiment is as follows Figure 4 As shown, observe Figure 4 It can be seen that the prepared MOF particles have a spherical structure with a particle size of about 2 μm.
[0059] According to the ionic conductivity formula: ionic conductivity L is the electrolyte thickness, R is the impedance, and S is the electrolyte area. The ionic conductivity of the composite polymer solid electrolyte at room temperature is calculated to be 2.5×10 -5 S cm -1 .
[0060] Comparative Example:
[0061] The difference of this comparative example is that the prepared solid electrolyte is a pure PEO-based polymer solid electrolyte without any filler added, and the electrochemical performance test of the assembled mold battery is carried out. The test conditions are that the charge and discharge cut-off voltage is 2.5-4.1V, the test current is 0.5C (1C = 170mAh g -1 ).
[0062] The composite polymer solid electrolyte matched in this embodiment is the same as that in embodiment 1. The test conditions are as follows: the charge and discharge cut-off voltage is 2.5-4.1V, the test current is 0.5C (1C = 170mAh g -1 ).
[0063] The polymer solid electrolyte material prepared in this embodiment is used in a polymer solid battery. The first charge and discharge curve under 0.5C and 2.5-4.1V conditions is as follows: Figure 5 As shown. Figure 5 It can be seen that its first discharge capacity is 152mAh g -1 , the first coulombic efficiency is 97.2%.
[0064] The composite polymer solid electrolyte material prepared in this embodiment is used in polymer solid-state batteries. The cycle performance under 0.5C and 2.5-4.1V conditions is shown in the figure below: Figure 6 As shown. Figure 6 It can be seen that the material exhibits good cycle stability.
[0065] It should be understood that the above specific embodiments of the present invention are only used to illustrate or explain the principles of the present invention, and do not constitute a limitation of the present invention. Therefore, any modifications, equivalent substitutions, improvements, etc. made without departing from the spirit and scope of the present invention should be included in the protection scope of the present invention. In addition, the appended claims of the present invention are intended to cover all changes and modifications that fall within the scope and boundaries of the appended claims, or the equivalent forms of such scope and boundaries.
Claims
1. A method for preparing a novel composite polymer-based solid electrolyte, characterized in that: The method is: Step 1: dissolving a certain amount of zinc ion salt in a polar solvent to obtain solution A, and stirring evenly; Step 2: dissolving the organic ligand in a polar solvent to obtain solution B, and stirring evenly; Step 3: Slowly introduce solution A into solution B and stir evenly for 1 hour, then transfer to a reactor for hydrothermal reaction; Step 4: After the reaction time is up, the obtained solution is centrifuged to obtain the bottom particles and vacuum dry them to obtain white particles; Step 5: The white particles are removed by a Soxhlet extractor, and then the removed particles are placed in a vacuum drying oven to be fully dried to obtain a metal organic framework MOF; Step 6: dissolving the lithium salt, metal organic framework MOF and polymer substrate in a polar solvent in sequence and stirring evenly to obtain a homogeneous solution; Step 7: pouring the obtained uniform solution into a mold containing flexible fibers to form it uniformly; Step 8: Transfer the mold to an inert gas-protected glove box for drying and removing the organic solution; transfer the formed electrolyte membrane to a vacuum drying oven for thorough drying to obtain a new composite polymer-based solid electrolyte.
2. The preparation method according to claim 1, characterized in that: In step 1, the zinc ion salt is one of zinc acetate, zinc sulfate, and zinc nitrite, and the polar solvent is one of methanol and N-methylformamide; in step 2, the organic ligand is one of fluorine-containing imidazoles such as 4-fluoro-1H-imidazole and 4(5)-(trifluoromethyl)imidazole.
3. The preparation method according to claim 1, characterized in that: In step 3, the molar ratio of the organic ligand to the zinc ion salt is 1:2-4; the hydrothermal temperature is 120-160° C., and the time is 24-36 hours.
4. The preparation method according to claim 1, characterized in that: In step 4, the drying temperature is 60° C. and the drying time is 12 h.
5. The preparation method according to claim 1, characterized in that: In step 5, the Soxhlet extractor is used for impurity removal for 24 hours, the vacuum drying temperature is 100° C., and the drying time is 12 hours.
6. The preparation method according to claim 1, characterized in that: In step six, the lithium salt is one of LiTFSI, LiClO4, and LiFSI, the polymer substrate is one of polyethylene oxide (PEO), polytetrafluoroethylene (PVDF), and polymethyl methacrylate (PMMA), and the polar solvent is acetonitrile or dimethyl sulfoxide; in the homogeneous solution, the molar ratio of the lithium salt to the polymer substrate is 1:10, and the mass ratio of the metal organic framework MOF to the polymer substrate is 1 to 2:
10.
7. The preparation method according to claim 1, characterized in that: In step seven, the flexible fiber is one of non-woven fabric, polyacrylonitrile carbon nanofiber, and PI fiber.
8. The preparation method according to claim 1, characterized in that: In step eight, the solution is dried in the glove box for 12 hours at a temperature of 60 to 80° C.; the vacuum drying oven is dried at 60° C. for 10 to 15 hours.
9. A novel composite polymer-based solid electrolyte prepared by the preparation method according to any one of claims 1 to 8.
10. Use of a novel composite polymer-based solid electrolyte prepared by the preparation method according to any one of claims 1 to 8 in preparing a composite polymer-based solid-state battery, characterized in that: The composite polymer-based solid-state battery is assembled from materials including a lithium negative electrode, a composite polymer-based solid electrolyte material, and a positive electrode material; the positive electrode material is one of high-voltage positive electrode materials such as LiFePO4, LiCoO2, and NCM811.