Foam sheet and adhesive tape

By optimizing the structural parameters of the foam sheet, increasing the stress relaxation rate and reducing the compression strength, the floating problem caused by surface tolerance deviation is solved, and the follow-up ability and sealing performance of the adhesive tape are improved. It is suitable for electronic equipment with curved structures. .

CN119013335APending Publication Date: 2024-11-22SEKISUI CHEMICAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380027737.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-18
Filing Date
2023-03-20
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

When using foam sheets as sealing material or impact absorbing material, the adhesive tape is stuck in electronic equipment with curved surface structure, and floating problems are easily caused by curved surface tolerance deviation, which is difficult to effectively solve in the prior art.

Method used

By increasing the stress relaxation rate of the foam sheet and reducing the compression strength, the structural parameters of the foam sheet are optimized, such as stress relaxation rate ≥23%, 25% compression strength ≤1000kPa, interlayer strength ≥0.6MPa, and closed porosity ≥≥≥≥≥≥≥≥≥≥≥≥≥≥≥≥≥≥≥≥≥≥≥≥≥≥≥≥≥≥≥≥≥≥≥≥≥≥≥≥≥≥≥≥≥≥≥≥≥≥≥≥≥≥≥≥≥ with stress relaxation rate 80%, gel fraction 30-80%, bubble flatness ≥2, density 0.05-0.6g/cm3, thickness 0.03-2mm, maximum temperature of dynamic viscoelastic loss tangent is 15-50℃, to prepare Foam sheet with permanent deformation.

Benefits of technology

It effectively suppresses the problem of floating on fixed components, improves the adherence and sealing performance of the adhesive tape, and is suitable for electronic equipment with curved structures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119013335A_ABST
    Figure CN119013335A_ABST
Patent Text Reader

Abstract

The foam sheet according to the present invention has a stress relaxation rate of 23% or more and a 25% compressive strength of 1000 kPa or less. The pressure-sensitive adhesive tape is provided with the foam sheet and a pressure-sensitive adhesive material provided on at least one surface of the multi-layer foam sheet. According to the present invention, it is possible to provide a foam sheet capable of increasing permanent deformation and an adhesive tape using the foam sheet.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a foam sheet and a pressure-sensitive adhesive tape including the foam sheet. Background Art

[0002] Adhesive tapes using foam sheets are widely used as sealing materials or shock absorbing materials in electronic devices such as mobile phones, cameras, displays, game consoles, electronic notebooks, and personal computers. As a foam used in an adhesive tape used as such a sealing material or shock absorbing material, for example, an acrylic foam described in Patent Document 1 is known. An adhesive tape using such an acrylic foam can be suitably used as a sealing material or a shock absorbing material.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application No. 2012-519750 Summary of the invention

[0006] Problems to be solved by the invention

[0007] In recent years, electronic devices with curved structures are being sold from the perspective of design. In such electronic devices, when an adhesive tape using a foam sheet is used as a sealing material or a shock absorbing material, the adhesive tape is sometimes attached to a curved surface to fix the component. In this case, the adhesive tape needs to be flexible in order to follow the curved surface, but due to the deviation of the curved surface tolerance, sometimes floating and other problems occur on the fixed component.

[0008] The inventors have conducted intensive research to solve the above problems and found that in addition to making the foam sheet soft, further increasing its permanent deformation can solve the floating of the fixed member and other problems. Therefore, the subject of the present invention is to provide a foam sheet capable of increasing permanent deformation and an adhesive tape using the foam sheet.

[0009] Means of solving problems

[0010] The present inventors have conducted intensive research on the permanent deformation of foam sheets and have found that the above-mentioned problems can be solved by increasing the stress relaxation rate of the foam sheets and reducing the 25% compression strength, thereby completing the following present invention.

[0011] That is, the present invention provides the following [1] to

[10] .

[0012] [1] A foamed sheet having a stress relaxation rate of 23% or more and a 25% compressive strength of 1000 kPa or less.

[0013] [2] The foam sheet according to [1] above, wherein the interlaminar strength is 0.6 MPa or more.

[0014] [3] The foam sheet according to [1] or [2] above, wherein the closed cell ratio is 80% or more.

[0015] [4] The foam sheet according to any one of [1] to [3] above, wherein the gel fraction is 30 to 80%.

[0016] [5] The foam sheet according to any one of [1] to [4], wherein the larger of the MD flatness and the TD flatness of the cells is 2 or more.

[0017] [6] The foam sheet according to any one of [1] to [5] above, wherein the density is 0.05 to 0.6 g / cm 3 .

[0018] [7] The foam sheet according to any one of [1] to [6] above, wherein the foam sheet has a thickness of 0.03 to 2 mm.

[0019] [8] The foam sheet according to any one of [1] to [7] above, wherein the foam sheet has at least one temperature showing a maximum value of the loss tangent (tan δ) of dynamic viscoelasticity in the range of 15 to 50°C.

[0020] [9] The foam sheet according to any one of [1] to [8] above, wherein the maximum value of the loss tangent (tan δ) of the dynamic viscoelasticity is 0.2 or more.

[0021]

[10] A pressure-sensitive adhesive tape comprising the foam sheet according to any one of [1] to [9] above and a pressure-sensitive adhesive material provided on at least one surface of the foam sheet.

[0022] Effects of the Invention

[0023] According to the present invention, a foam sheet capable of increasing permanent deformation and a pressure-sensitive adhesive tape using the foam sheet can be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 It is a schematic diagram showing the measuring device of interlaminar strength. DETAILED DESCRIPTION

[0025] Hereinafter, the present invention will be described in detail using embodiments.

[0026] [Foaming sheet]

[0027] The foam sheet of the present invention has a stress relaxation rate of 23% or more and a 25% compression strength of 1000 kPa or less. Thus, the permanent deformation of the foam sheet can be increased. Furthermore, even if a curved surface to which an adhesive tape using the foam sheet is attached is adhered, even if there is a tolerance of the curved surface, it is possible to suppress the occurrence of problems such as floating in the component fixed by the adhesive tape.

[0028] (Stress relaxation rate)

[0029] The stress relaxation rate of the foam sheet of the present invention is 23% or more. If the stress relaxation rate of the foam sheet is less than 23%, the permanent deformation of the foam sheet becomes insufficient, and sometimes the foam sheet cannot fully alleviate the deviation of the curved surface tolerance. As a result, problems such as floating sometimes occur in components fixed with an adhesive tape using a foam sheet. From this perspective, the stress relaxation rate of the foam sheet of the present invention is preferably 25% or more, more preferably 27% or more, further preferably 30% or more, further preferably 33% or more, and further preferably 35% or more. The upper limit of the range of the stress relaxation rate of the foam sheet of the present invention is not particularly limited, and is 60% from the perspective of sealing. It should be noted that the stress relaxation rate of the foam sheet can be measured by the method described in the embodiments described later. In addition, the stress relaxation rate of the foam sheet can be controlled by adjusting the type and proportion of the resin constituting the foam sheet, the flatness of the bubbles, the thickness of the foam sheet, the density of the foam sheet, the maximum value of the loss tangent (tanδ) of the dynamic viscoelasticity of the foam sheet and the temperature showing the maximum value (glass transition temperature (Tg)), etc.

[0030] (25% compression strength)

[0031] The 25% compressive strength of the foam sheet of the present invention is 1000kPa or less. If the 25% compressive strength of the foam sheet is greater than 1000kPa, the foam sheet may not be able to fully follow the curved surface. As a result, problems such as the tape peeling off from the component fixed by the adhesive tape using the foam sheet may occur. From this perspective, the 25% compressive strength of the foam sheet is preferably 700kPa or less, more preferably 500kPa or less, and further preferably 200kPa or less. The lower limit of the range of the 25% compressive strength of the foam sheet of the present invention is not particularly limited, and is usually 5kPa. It should be noted that the 25% compressive strength of the foam sheet can be measured by the method described in the embodiments described later. In addition, the 25% compressive strength of the foam sheet can be controlled by adjusting the type and proportion of the resin constituting the foam sheet, the flatness of the bubbles, the thickness of the foam sheet, the density of the foam sheet, the maximum value of the loss tangent (tanδ) of the dynamic viscoelasticity of the foam sheet, and the temperature (glass transition temperature (Tg)) showing the maximum value.

[0032] (Interlaminar strength)

[0033] The interlaminar strength of the foam sheet of the present invention is preferably 0.6MPa or more. If the interlaminar strength of the foam sheet is 0.6MPa or more, when the foam sheet is used for the adhesive tape, the strength of the adhesive tape can be improved, and as a result, the adhesive tape can be suppressed from being damaged by an impact from the outside. From this perspective, the interlaminar strength of the foam sheet is more preferably 1.0MPa or more, and more preferably 1.5MPa or more. The upper limit of the range of the interlaminar strength of the foam sheet of the present invention is not particularly limited, and is usually 10MPa. It should be noted that the interlaminar strength of the foam sheet can be measured by the method described in the embodiments described later. In addition, the interlaminar strength of the foam sheet can be controlled by adjusting the type and ratio of the resin constituting the foam sheet, the flatness of the bubble, the thickness of the foam sheet, the density of the foam sheet, the maximum value of the loss tangent (tanδ) of the dynamic viscoelasticity of the foam sheet and the temperature (glass transition temperature (Tg)) showing the maximum value.

[0034] (Closed Porosity)

[0035] The closed cell rate of the foam sheet of the present invention is preferably 80% or more. If the closed cell rate of the foam sheet is 80% or more, the dustproofness and water resistance of the foam sheet can be improved when the foam sheet is used as a sealing material. From this perspective, the closed cell rate of the foam sheet is more preferably 90% or more, and further preferably 95% or more. The upper limit of the range of the closed cell rate of the foam sheet of the present invention is not particularly limited, and is usually 100%. It should be noted that the closed cell rate of the foam sheet can be measured by the method described in the embodiments described later.

[0036] (Gel fraction)

[0037] The gel fraction of the foam sheet of the present invention is preferably 30 to 80%. If the gel fraction of the foam sheet is 30 to 80%, the bubbles in the foam sheet can be reduced and the interlayer strength can be improved. From this perspective, the gel fraction of the multilayer foam sheet is more preferably 35 to 70%, and further preferably 40 to 65%. It should be noted that the gel fraction of the foam sheet can be measured by the method described in the examples described below.

[0038] (Flattening ratio of bubbles)

[0039] In the MD flatness and TD flatness of the bubbles in the foam sheet of the present invention, the larger one is preferably 2 or more. It should be noted that in this specification, "MD" refers to the longitudinal direction (machine direction), which is a direction consistent with the extrusion direction of the sheet, etc. "TD" refers to the transverse direction, which is a direction orthogonal to the MD and parallel to the surface of the sheet. If the larger one of the MD flatness and TD flatness of the bubble is 2 or more, the restoring force of the bubble in the thickness direction can be suppressed, thereby making it easy to make the stress relaxation rate of the foam sheet 23% or more. From this point of view, the larger one of the MD flatness and TD flatness of the bubble is more preferably 3 or more, and further preferably 4 or more. It should be noted that the MD flatness and TD flatness of the bubbles in the foam sheet can be measured by the method described in the embodiments described later. In addition, in the manufacture of the foam sheet, the MD flatness and TD flatness of the bubbles in the foam sheet can be adjusted by stretching the foam sheet in at least one direction of MD and TD. Furthermore, from the viewpoint of the stress relaxation rate of the foamed sheet, it is more preferred that both the MD flatness ratio and the TD flatness ratio of the cells are 2 or more.

[0040] (Average bubble diameter)

[0041] The average bubble diameter of the foam sheet of the present invention is preferably 5 to 400 μm. As described later, the foam sheet can be used in any shape, but is preferably narrow. If the average bubble diameter of the foam sheet is 10 to 300 μm, even if the foam sheet is narrow, sufficient waterproofness of the foam sheet can be ensured. From this perspective, the average bubble diameter of the foam sheet of the present invention is more preferably 10 to 250 μm, and further preferably 10 to 200 μm. It should be noted that the average bubble diameter of the foam sheet can be measured by the method described in the embodiments described later, and the average bubble diameter referred to here refers to the average value of the average bubble diameters of MD and TD.

[0042] (density)

[0043] The density of the foam sheet of the present invention is preferably 0.05 to 0.6 g / cm 3 If the density of the foam sheet is 0.05-0.6 g / cm 3 , it is easier to make the stress relaxation rate of the foam sheet more than 23% and the 25% compression strength of the foam sheet less than 1000 kPa. From this perspective, the density of the foam sheet of the present invention is more preferably 0.07 to 0.57 g / cm 3 , more preferably 0.10 to 0.55 g / cm 3 It should be noted that the density of the foam sheet can be measured by the method described in the examples described below.

[0044] (Foaming ratio)

[0045] The foaming ratio of the foam sheet of the present invention is preferably 1.5 times or more. If the foaming ratio of the foam sheet is 1.5 times or more, it is easier to make the stress relaxation rate of the foam sheet 23% or more and make the 25% compression strength of the foam sheet 1000kPa or less. From this perspective, the foaming ratio of the foam sheet of the present invention is more preferably 4 times or more, and further preferably 5 times or more. The upper limit of the range of the foaming ratio of the foam sheet of the present invention is not particularly limited, and is generally 30 times, preferably 20 times. It should be noted that the foaming ratio of the foam sheet can be measured by the method described in the examples described later.

[0046] (thickness)

[0047] The thickness of the foam sheet of the present invention is preferably 0.03 to 2 mm. If the thickness of the foam sheet is 0.03 to 2 mm, it is easier to make the stress relaxation rate of the foam sheet 23% or more and the 25% compression strength of the foam sheet 1000 kPa or less. From this perspective, the thickness of the foam sheet of the present invention is more preferably 0.05 to 1.5 mm, and further preferably 0.07 to 1 mm. It should be noted that the thickness of the foam sheet can be measured by the method described in the examples described below.

[0048] (Loss tangent (tanδ))

[0049] The foam sheet of the present invention preferably has at least one temperature showing a maximum value of the loss tangent (tanδ) of dynamic viscoelasticity in the range of 15 to 50°C. If the foam sheet has at least one temperature showing a maximum value of tanδ of dynamic viscoelasticity in the range of 15 to 50°C, it is easier to make the stress relaxation rate of the foam sheet 23% or more. From this perspective, it is more preferred that at least one temperature showing a maximum value of the loss tangent (tanδ) of dynamic viscoelasticity exists in the range of 15 to 47°C, and it is further preferred that at least one temperature exists in the range of 23 to 43°C. It should be noted that the tanδ of the foam sheet is the loss tangent obtained by measuring the dynamic viscoelasticity at a measurement frequency of 10 Hz. Tanδ is the ratio (G" / G') of the storage shear elastic modulus (G') to the loss shear elastic modulus (G"), which indicates how much energy (converted into heat) the material absorbs when the material is deformed. It should be noted that the temperature showing a maximum value of the loss tangent (tanδ) of the dynamic viscoelasticity of the foam sheet is usually the glass transition temperature (Tg) of the foam sheet.

[0050] In addition, the maximum value of the loss tangent (tanδ) of the foam sheet of the present invention is preferably greater than 0.2. If the tanδ of the foam sheet is greater than 0.2, it is easier to make the stress relaxation rate of the foam sheet greater than 23%. From this perspective, the maximum value of tanδ of the foam sheet of the present invention is more preferably greater than 0.3, and further preferably greater than 0.4. In addition, the upper limit value of the range of the maximum value of tanδ of the foam sheet of the present invention is not particularly limited, and is usually 3. It should be noted that with respect to the maximum value mentioned here, the temperature showing the maximum value can be in the range of 15 to 50°C.

[0051] It should be noted that the maximum value of tan δ of the foam sheet and the temperature at which the maximum value is shown can be measured by the method described in the examples described later. In addition, the maximum value of tan δ of the foam sheet, the number of maximum values ​​of tan δ and the temperature at which the maximum value of tan δ is shown can be controlled by adjusting the type and ratio of the resin constituting the foam sheet, the flatness of the bubbles, the thickness of the foam sheet, the density of the foam sheet, etc.

[0052] [Resin constituting the foam sheet]

[0053] The foam sheet of the present invention may contain an elastomer (A), preferably an elastomer (A) and a polyolefin resin (B). By using an elastomer and a polyolefin resin, the stress relaxation rate of the foam sheet can be easily made 23% or more and the 25% compressive strength can be easily made 1000 kPa or less.

[0054] (Elastomer (A))

[0055] As elastomer (A), thermoplastic elastomer, ethylene-α-olefin copolymer rubber, amorphous 4-methyl-1-pentene copolymer, etc. can be cited. As thermoplastic elastomer, olefin thermoplastic elastomer, styrene thermoplastic elastomer, vinyl chloride thermoplastic elastomer, polyurethane thermoplastic elastomer, polyester thermoplastic elastomer, polyamide thermoplastic elastomer, etc. can be cited. Elastomer (A) can use one of these components alone, or two or more of them can be used in combination.

[0056] Among them, olefin-based thermoplastic elastomers, styrene-based thermoplastic elastomers, ethylene-α-olefin-based copolymer rubbers, and amorphous 4-methyl-1-pentene copolymers are preferred, styrene-based thermoplastic elastomers and amorphous 4-methyl-1-pentene copolymers are more preferred, and styrene-based thermoplastic elastomers are further preferred.

[0057] <Olefin thermoplastic elastomer>

[0058] Olefin thermoplastic elastomer (TPO) is a substance that generally uses polyolefins such as polyethylene and polypropylene as hard segments and rubber components such as butyl rubber, halogenated butyl rubber, EPDM (ethylene-propylene-diene rubber), EPM (ethylene-propylene rubber), NBR (acrylonitrile-butadiene rubber), and natural rubber as soft segments. As olefin thermoplastic elastomer (TPO), any of a blended type, a dynamically crosslinked type, and a polymerized type can be used.

[0059] Preferred specific examples of the rubber component include the above-mentioned EPM and EPDM, and EPDM is particularly preferred. It should be noted that, as EPDM, ethylene-propylene-5-ethylidene-2-norbornene copolymer rubber and ethylene-propylene-dicyclopentadiene copolymer rubber can be listed, among which ethylene-propylene-dicyclopentadiene copolymer rubber is preferred.

[0060] In addition, as olefin-based thermoplastic elastomer, block copolymer type can be cited. As block copolymer type, block copolymers with crystalline blocks and soft segment blocks can be cited, more specifically, crystalline olefin block-ethylene butene copolymer-crystalline olefin block copolymer (CEBC) can be exemplified. In CEBC, crystalline olefin block is preferably crystalline ethylene block, and as a commercially available product of such CEBC, " DYNARON 6200P " manufactured by JSR Co., Ltd. can be cited.

[0061] <Styrene-based thermoplastic elastomer>

[0062] Examples of the styrene-based thermoplastic elastomer include block copolymers having a polymer or copolymer block of styrene and a polymer or copolymer block of a conjugated diene compound, etc. Examples of the conjugated diene compound include isoprene and butadiene.

[0063] The styrene-based thermoplastic elastomer used in the present invention may or may not be hydrogenated, but is preferably hydrogenated. When hydrogenated, the hydrogenation can be performed by a known method.

[0064] As styrene-based thermoplastic elastomers, block copolymers are generally used, and examples thereof include styrene-isoprene block copolymers (SI), styrene-isoprene-styrene block copolymers (SIS), styrene-butadiene block copolymers (SB), styrene-butadiene-styrene block copolymers (SBS), styrene-ethylene / butylene-styrene block copolymers (SEBS), styrene-ethylene / propylene-styrene block copolymers (SEPS), styrene-ethylene / ethylene / propylene-styrene block copolymers (SEEPS), styrene-ethylene / butylene block copolymers (SEB), styrene-ethylene / propylene block copolymers (SEP), styrene-ethylene / butylene-crystalline olefin block copolymers (SEBC), and the like.

[0065] As the styrene-based thermoplastic elastomer, block copolymers are preferred, among which SIS, SEBS, SEPS, SEEPS, and SEBC are more preferred, SEEPS and SEBS are further preferred, and SIS and SEBS are particularly preferred.

[0066] It should be noted that commercially available products of SIS include "HiBla (registered trademark) 5125" (styrene content 20% by mass, Tg = -13°C) and "HiBla (registered trademark) 5127" (styrene content 20% by mass, Tg = 8°C) manufactured by Kuraray Co., Ltd. Commercially available products of SEBS include the TAFTEC (registered trademark) series and SOE (registered trademark) series manufactured by Asahi Kasei Corporation.

[0067] Styrene-based thermoplastic elastomers, by having structural units derived from styrene, can make the impact resistance of the foam sheet good. The styrene content in the styrene-based thermoplastic elastomer is preferably 5 to 50% by mass. By setting the styrene content to this range, excellent impact resistance can be obtained. In addition, by being set to below the above upper limit, the compatibility with the polyolefin resin (B) described in detail later becomes good, and the crosslinking and foaming properties tend to become good. Considering these aspects, the styrene content in the styrene-based thermoplastic elastomer is more preferably 7 to 40% by mass, and further preferably 7 to 30% by mass.

[0068] The number average molecular weight of the styrene-based thermoplastic elastomer is not particularly limited, but is preferably 30,000 to 800,000, more preferably 120,000 to 180,000, from the viewpoint of breaking strength and processability.

[0069] In addition, the number average molecular weight is a polystyrene conversion value measured using gel permeation chromatography (GPC).

[0070] <Ethylene-α-olefin copolymer rubber>

[0071] Examples of the α-olefin used in the ethylene-α-olefin copolymer rubber include one or more α-olefins having 3 to 15 carbon atoms, preferably 3 to 10 carbon atoms, such as propylene, 1-butene, 2-methylpropylene, 3-methyl-1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, and 1-octene. Among them, propylene and 1-butene are preferred, and 1-butene is more preferred.

[0072] The ethylene-α-olefin copolymer rubber used herein is an amorphous or low-crystalline rubber material obtained by substantially random copolymerization of two or more olefin monomers.

[0073] The ethylene-α-olefin copolymer rubber may have other monomer units in addition to the ethylene unit and the α-olefin unit.

[0074] Examples of the monomers forming the other monomer units include conjugated dienes having 4 to 8 carbon atoms such as 1,3-butadiene, 2-methyl-1,3-butadiene (isoprene), 1,3-pentadiene, and 2,3-dimethyl-1,3-butadiene, non-conjugated dienes having 5 to 15 carbon atoms such as dicyclopentadiene, 5-ethylidene-2-norbornene, 1,4-hexadiene, 1,5-dicyclooctadiene, 7-methyl-1,6-octadiene, and 5-vinyl-2-norbornene, vinyl ester compounds such as vinyl acetate, unsaturated carboxylic acid esters such as methyl acrylate, ethyl acrylate, butyl acrylate, methyl methacrylate, and ethyl methacrylate, and unsaturated carboxylic acids such as acrylic acid and methacrylic acid. These monomers may be used alone or in combination of two or more. Among them, non-conjugated dienes having 5 to 15 carbon atoms are preferred, and 5-ethylidene-2-norbornene, 1,4-hexadiene, and dicyclopentadiene (DCPD) are more preferred in view of availability.

[0075] The content of ethylene units in the ethylene-α-olefin copolymer rubber is usually 30 to 85% by mass, preferably 40 to 80% by mass, and more preferably 45 to 75% by mass. In addition, the content of α-olefin units having 3 to 15 carbon atoms, preferably 3 to 10 carbon atoms, such as propylene, is usually 10 to 60% by mass, preferably 15 to 50% by mass. The content of other monomer units such as non-conjugated dienes is usually 0 to 20% by mass, preferably 1 to 10% by mass.

[0076] As the ethylene-α-olefin copolymer rubber, terpolymers such as EPDM (ethylene-propylene-diene rubber) and EBDM (ethylene-butene-1-diene rubber) are preferred. As the ethylene-α-olefin copolymer, "EBT K-9330" manufactured by Mitsui Chemicals, Inc. is exemplified.

[0077] <Amorphous 4-methyl-1-pentene copolymer>

[0078] As the amorphous 4-methyl-1-pentene copolymer, there can be mentioned a copolymer of 4-methyl-1-pentene and an α-olefin other than 4-methyl-1-pentene. As the α-olefin, for example, there can be mentioned an α-olefin having 2 to 20 carbon atoms, preferably ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 1-decene, and more preferably ethylene, propylene, etc. Among them, a 4-methyl-1-pentene / propylene copolymer is preferred.

[0079] Examples of the amorphous 4-methyl-1-pentene copolymer include "EP1001" and "EP1013" manufactured by Mitsui Chemicals, Inc.

[0080] (Polyolefin resin (B))

[0081] The polyolefin resin is a thermoplastic resin. Specific examples thereof include polyethylene resin, polypropylene resin, polybutene resin, and ethylene-vinyl acetate copolymer. Among them, polyethylene resin is preferred.

[0082] In addition, as the polyethylene resin, low-density polyethylene (LDPE) is preferred, and linear low-density polyethylene (LLDPE) is more preferred. Therefore, it is particularly preferred to use a styrene-based thermoplastic elastomer as the elastomer (A) and LLDPE as the polyolefin resin (B).

[0083] Furthermore, examples of the polyethylene resin include polyethylene resins polymerized using a polymerization catalyst such as a Ziegler-Natta catalyst, a metallocene catalyst, and a chromium oxide compound, and polyethylene resins polymerized using a metallocene catalyst are preferably used.

[0084] (Metallocene Catalyst)

[0085] As metallocene catalysts, compounds such as bis(cyclopentadienyl) metal complexes having a structure in which a transition metal is sandwiched between π-electron unsaturated compounds can be cited. More specifically, compounds in which one or more cyclopentadienyl rings or their analogs exist as ligands on tetravalent transition metals such as titanium, zirconium, nickel, palladium, hafnium and platinum can be cited.

[0086] The active points of the metallocene catalyst are uniform in nature, and each active point has the same degree of activity. The polymer synthesized using the metallocene catalyst has high uniformity in molecular weight, molecular weight distribution, composition, composition distribution, etc., so when a sheet containing a polymer synthesized using the metallocene catalyst is cross-linked, the cross-linking is uniformly performed. The uniformly cross-linked sheet is uniformly foamed, so it is easy to stabilize the physical properties. In addition, since it can be uniformly stretched, the thickness of the foam can be made uniform.

[0087] As the ligand, for example, a cyclopentadienyl ring, an indenyl ring, etc. can be cited. These cyclic compounds can be substituted by a hydrocarbon group, a substituted hydrocarbon group, or a hydrocarbon-substituted metalloid group. As the hydrocarbon group, for example, a methyl group, an ethyl group, various propyl groups, various butyl groups, various pentyl groups, various hexyl groups, 2-ethylhexyl groups, various heptyl groups, various octyl groups, various nonyl groups, various decyl groups, various cetyl groups, phenyl groups, etc. can be cited. It should be noted that "various" refers to various isomers including normal, secondary, tertiary, and iso.

[0088] Furthermore, a ligand obtained by polymerizing a cyclic compound into an oligomer may be used.

[0089] Furthermore, in addition to the π-electron unsaturated compounds, monovalent anionic ligands such as chlorine and bromine, divalent anionic chelate ligands, hydrocarbons, alkoxides, arylamides, aryloxides, amides, phosphides, arylphosphides, etc. can also be used.

[0090] Examples of the metallocene catalyst containing a tetravalent transition metal and a ligand include cyclopentadienyl titanium tris(dimethylamide), methylcyclopentadienyl titanium tris(dimethylamide), bis(cyclopentadienyl)titanium dichloride, and dimethylsilyltetramethylcyclopentadienyl-tert-butylamide zirconium dichloride.

[0091] Metallocene catalysts act as catalysts in the polymerization of various olefins by combining with specific co-catalysts (co-catalysts). Specific co-catalysts include methylaluminoxane (MAO), boron compounds, etc. It should be noted that the ratio of the co-catalyst to the metallocene catalyst is preferably 100,000 to 1,000,000 mole times, more preferably 500,000 to 5,000 mole times.

[0092] In addition, as polyethylene resin, linear low-density polyethylene is preferred. The linear low-density polyethylene is more preferably a linear low-density polyethylene obtained by copolymerizing ethylene (for example, 75% by mass or more, preferably 90% by mass or more relative to the total monomer amount) with a small amount of α-olefin as required. As α-olefin, specifically, propylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-heptene and 1-octene can be cited. Among them, α-olefins with 4 to 10 carbon atoms are preferred.

[0093] From the viewpoint of flexibility, the density of the polyethylene resin, for example, the above-mentioned linear low-density polyethylene, is preferably 0.870 to 0.925 g / cm 3 , more preferably 0.890 to 0.925 g / cm 3 , more preferably 0.910 to 0.925 g / cm 3As the polyethylene resin, a plurality of polyethylene resins may be used, and polyethylene resins having a density outside the above-mentioned range may be added.

[0094] Examples of the ethylene-vinyl acetate copolymer used as the polyolefin-based resin include ethylene-vinyl acetate copolymers containing 50% by mass or more of ethylene.

[0095] In addition, as the polypropylene resin, for example, homopolypropylene, propylene-α-olefin copolymer containing 50% by mass or more of propylene, etc. can be listed. These can be used alone or in combination of two or more. As the α-olefin constituting the propylene-α-olefin copolymer, specifically, ethylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-heptene, 1-octene, etc. can be listed, among which α-olefins with 6 to 12 carbon atoms are preferred.

[0096] Examples of the polybutene resin include homopolymers of butene-1 and copolymers thereof with ethylene or propylene.

[0097] [Mass ratio of elastomer (A) to polyolefin resin (B)]

[0098] The mass ratio of the elastomer (A) to the polyolefin resin (B) is preferably 90:10 to 20:80. If it is within this range, it is possible to easily manufacture a foam sheet that can exert the effects of the present invention. From the perspective of obtaining a more effective foam sheet, the mass ratio of the (A) component to the (B) component is more preferably in the range of 80:20 to 25:75, more preferably in the range of 75:25 to 30:70, and even more preferably in the range of 70:30 to 50:50.

[0099] The foam sheet of the present invention may contain resins other than the elastomer (A) and the polyolefin resin (B) within a range that does not hinder the effect of the present invention. However, from the perspective of making the stress relaxation rate of the foam sheet 23% or more and making the 25% compression strength 1000 kPa or less, it is preferred that the total ratio of the elastomer (A) and the polyolefin resin (B) in the resin component of the foam sheet of the present invention is high. Specifically, the total ratio of the elastomer (A) and the polyolefin resin (B) in the resin component of the foam sheet of the present invention is preferably 80 to 100% by mass, more preferably 90 to 100% by mass, further preferably 95 to 100% by mass, and further preferably 99 to 100% by mass.

[0100] [additive]

[0101] The foam sheet of the present invention is preferably obtained by foaming a foamable composition containing the above-mentioned resin and a foaming agent. The foaming agent is preferably a thermally decomposable foaming agent.

[0102] As the thermal decomposition type foaming agent, an organic foaming agent or an inorganic foaming agent can be used. Examples of the organic foaming agent include azodicarbonamide, azodicarboxylic acid metal salts (barium azodicarboxylate, etc.), azo compounds such as azobisisobutyronitrile, nitroso compounds such as N,N'-dinitrosopentamethylenetetramine, hydrazinedicarbonamide, 4,4'-oxybis(benzenesulfonylhydrazide), hydrazine derivatives such as toluenesulfonylhydrazide, and semicarbazide compounds such as toluenesulfonylsemicarbazide.

[0103] Examples of the inorganic foaming agent include ammonium carbonate, sodium carbonate, ammonium hydrogen carbonate, sodium hydrogen carbonate, ammonium nitrite, sodium borohydride, and anhydrous monosodium citrate.

[0104] Among them, azo compounds are preferred, and azodicarbonamide is more preferred, from the viewpoints of obtaining fine bubbles, economic efficiency, and safety.

[0105] The thermal decomposition type foaming agent may be used alone or in combination of two or more.

[0106] The amount of the foaming agent in the foamable composition relative to 100 parts by mass of the resin is preferably 1 to 20 parts by mass, more preferably 1.5 to 15 parts by mass, and further preferably 3 to 10 parts by mass. By making the amount of the foaming agent more than 1 part by mass, the foamable sheet is appropriately foamed, and appropriate softness and impact absorption can be given to the foam sheet. In addition, by making the amount of the foaming agent less than 20 parts by mass, it is possible to prevent the foam sheet from being excessively foamed, so that the mechanical strength of the foam sheet is good.

[0107] A decomposition temperature regulator may be added to the foamable composition. The decomposition temperature regulator is added as a substance having a regulating function such as lowering the decomposition temperature of the thermal decomposition type foaming agent or accelerating the decomposition rate. Specific compounds include zinc oxide, zinc stearate, urea, etc. In order to adjust the surface state of the foam sheet, for example, 0.01 to 5 parts by mass of the decomposition temperature regulator is added relative to 100 parts by mass of the resin.

[0108] An antioxidant may be added to the foamable composition. Examples of the antioxidant include phenolic antioxidants such as 2,6-di-tert-butyl-p-cresol, sulfur antioxidants, phosphorus antioxidants, and amine antioxidants. The antioxidant may be added in an amount of, for example, 0.01 to 5 parts by mass relative to 100 parts by mass of the resin.

[0109] In addition to the above, additives commonly used in foams, such as a heat stabilizer, a colorant, a flame retardant, an antistatic agent, and a filler, may be formulated in the foamable composition.

[0110] In the foam sheet, the elastomer (A) and the polyolefin resin (B) are the main components, and the total content of the components (A) and (B) is, for example, 70% by mass or more, preferably 80% by mass or more, and more preferably 90% by mass or more, based on the total amount of the foam sheet.

[0111] [Method for producing foam sheet]

[0112] The foam sheet of the present invention is not particularly limited and can be produced by heating a foam sheet formed of a foamable composition containing at least a resin and a thermally decomposable foaming agent to foam the thermally decomposable foaming agent. In addition, the foam sheet is preferably cross-linked and the cross-linked foam sheet is heated to foam.

[0113] More specifically, the method for producing the foam sheet preferably includes the following steps (1) to (3).

[0114] Step (1): a step of molding a foamable sheet formed from a foamable composition containing at least a resin and a thermally decomposable foaming agent.

[0115] Step (2): A step of irradiating the foamable sheet with ionizing radiation to crosslink the foamable sheet.

[0116] Step (3): A step of heating the cross-linked foamable sheet to foam the thermally decomposable foaming agent to obtain a foamed sheet.

[0117] In step (1), the method for molding the foamable sheet is not particularly limited. For example, the resin and the additive are supplied to an extruder for melt kneading, and the foamable composition is extruded from the extruder into a sheet for molding. In addition, the foamable sheet can also be molded by pressing the foamable composition. The molding temperature of the foamable sheet (i.e., the temperature during extrusion or the temperature during pressing) is preferably 50 to 250°C, more preferably 80 to 180°C.

[0118] As a method for crosslinking the foamable composition in step (2), a method of irradiating the foamable sheet with ionizing radiation such as electron beams, α-rays, β-rays, and γ-rays is used. The irradiation amount of the above-mentioned ionizing radiation can be adjusted so that the crosslinking degree of the obtained foam sheet is within the above-mentioned desired range, and is preferably 1 to 12 Mrad, and more preferably 1.5 to 10 Mrad.

[0119] In step (3), the heating temperature when heating the foamable composition to foam the thermally decomposable foaming agent may be equal to or higher than the foaming temperature of the thermally decomposable foaming agent, and is preferably 200 to 300° C., more preferably 220 to 280° C. In step (3), the foamable composition is foamed to form bubbles and a foam.

[0120] In the present production method, the foam sheet may be thinned by calendering, stretching or the like, and the cell flatness ratio may be adjusted by calendering, stretching or the like.

[0121] However, the present manufacturing method is not limited to the above method, and the foam sheet can also be obtained by methods other than the above method. For example, instead of irradiating ionizing radiation, crosslinking can be performed by pre-mixing an organic peroxide in the foamable composition and heating the foamable sheet to decompose the organic peroxide.

[0122] When cross-linking is not required, step (2) may be omitted. In this case, in step (3), the uncross-linked foamable sheet may be heated to be foamed.

[0123] [Adhesive tape]

[0124] The adhesive tape of the present invention comprises the foam sheet of the present invention and an adhesive material disposed on at least one surface of the foam sheet. The adhesive tape can be bonded to other members such as a supporting member via the adhesive material. The adhesive tape may be an adhesive tape having adhesive materials disposed on both sides of the foam sheet or an adhesive tape having adhesive materials disposed on one side.

[0125] In addition, as long as the adhesive material has at least an adhesive layer, it can be a single adhesive layer stacked on the surface of the foam sheet, or a double-sided adhesive sheet attached to the surface of the foam sheet, preferably a single adhesive layer. It should be noted that the double-sided adhesive sheet has a substrate and an adhesive layer arranged on both sides of the substrate. The double-sided adhesive sheet is used to bond one adhesive layer to the foam sheet and the other adhesive layer to other components.

[0126] The adhesive constituting the adhesive layer is not particularly limited, and examples thereof include acrylic adhesives, urethane adhesives, rubber adhesives, silicone adhesives, etc. In addition, a release sheet such as release paper may be further attached to the adhesive material.

[0127] The thickness of the adhesive layer is preferably 5 to 200 μm, more preferably 7 to 150 μm, and even more preferably 10 to 100 μm.

[0128] [Foam sheet roll]

[0129] The foam sheet of the present invention can be formed into a roll. By forming a roll, storage becomes easy and transportation is also convenient. It should be noted that when in use, it can be rolled out from a roll and used. As mentioned above, the stress relaxation rate of the foam sheet of the present invention is more than 23%, so when the foam sheet is rolled into a roll, the occurrence of problems such as wrinkles can be suppressed. In addition, the 25% compression strength of the foam sheet of the present invention is below a certain value as mentioned above, so when the foam sheet is rolled into a roll, the occurrence of undesirable conditions such as floating can be suppressed.

[0130] [Application of Foam Sheet]

[0131] The use of the foam sheet of the present invention is not particularly limited, and it is preferably used in electronic equipment applications. As electronic devices, portable electronic devices such as mobile phones such as smart phones, game consoles, electronic notepads, tablet terminals, notebook personal computers, etc. can be listed. The foam sheet can be used as a cushioning material inside the electronic device, and is preferably used as a cushioning material for display devices. In addition, it is also preferably used as a sealing material for filling gaps between components inside the electronic device. The foam sheet of the present invention can suppress the problem of floating on a fixed component due to the deviation of the curved surface tolerance, and is therefore more preferably used in an electronic device with a curved surface structure. Moreover, the foam sheet of the present invention is also preferably arranged along a component with a curved surface structure in an electronic device with a curved surface structure.

[0132] The foam sheet of the present invention can be used in any shape, for example, it can be used in a narrow width, specifically, it can be made into a slender rectangular shape, a frame shape such as a rectangular frame, an L shape, a U shape, etc. As their width, for example, it is less than 5 mm, preferably less than 3 mm, more preferably less than 1 mm, and for example, it is more than 0.1 mm.

[0133] The foam sheet used as a buffer material for a display device can be arranged, for example, on the back side of a display panel provided in various electronic devices to buffer the impact acting on the display panel. In this case, the foam sheet can be arranged on a supporting member arranged on the back side of the display panel. The supporting member, for example, constitutes a part of a housing of various electronic devices.

[0134] The foam sheet used in the electronic device can be provided with an adhesive material as described above, and can be bonded to a display panel, a supporting member, etc. using the adhesive material. The foam sheet of the present invention can suppress the problem of floating in a fixed member due to the deviation of the tolerance of the curved surface, and is therefore preferably used in a portion with a curved surface structure. Specifically, the foam sheet of the present invention can be bonded to a supporting member, a display panel, etc. with a curved surface structure by an adhesive material. Thus, even if there is a deviation of the curved surface tolerance in components such as a supporting component and a display panel, other components affixed to the component can be suppressed from floating, etc.

[0135] Example

[0136] The present invention will be described in more detail by way of examples, but the present invention is not limited to these examples.

[0137] [Measurement method]

[0138] The measuring methods and evaluation methods of various physical properties are as follows.

[0139] <Thickness>

[0140] Use a micrometer to measure.

[0141] <Density, expansion ratio>

[0142] The specific volume (unit: cc / g) of the foamed sheet before and after foaming was measured, and the foaming ratio was calculated by the specific volume after foaming / specific volume before foaming. The density was also calculated from the measured specific volume.

[0143] <Average cell diameter and cell flatness>

[0144] The foam sheet was cut along MD and TD in the thickness direction (ZD), and a 200-fold magnified photograph was taken using a digital microscope (manufactured by Keyence Co., Ltd., product name "VHX-900"). In the enlarged photograph taken, the bubble diameter of MD, the bubble diameter of TD, and the bubble diameter of ZD were measured for all bubbles present in the cut surface with a length of 2 mm for each of MD and TD, and the operation was repeated 5 times. Then, the average value of the bubble diameters of MD, TD, and ZD of all bubbles was taken as the average bubble diameter of MD, TD, and ZD. Then, the average value of the average bubble diameters of MD and TD was taken as the average bubble diameter. In addition, the MD flatness of the bubble was calculated by dividing the average bubble diameter of MD by the average bubble diameter of ZD. Furthermore, the TD flatness of the bubble was calculated by dividing the average bubble diameter of TD by the average bubble diameter of ZD.

[0145] <The maximum value of loss tangent (tanδ) and the temperature at which the maximum value of loss tangent (tanδ) appears>

[0146] The maximum value of tan δ and the temperature showing the maximum value of tan δ were determined using a tensile storage modulus measuring device manufactured by ITECH Instruments Co., Ltd. under the following measuring conditions. It should be noted that the temperature showing the maximum value of tan δ is generally equivalent to the glass transition temperature (Tg).

[0147] (Measurement conditions)

[0148] Length between marking lines: 2.5cm

[0149] Sample width: 0.5cm

[0150] Sample thickness: the thickness of the foam sheet

[0151] Deformation Mode: Stretch

[0152] Static / dynamic stress ratio: 1.5

[0153] Set deformation: 1.0%

[0154] Set heating speed: 10℃ / min

[0155] Measuring frequency 10Hz

[0156] Temperature range: -150℃~100℃

[0157] <25% compression strength>

[0158] The measurement was performed at a measurement temperature of 23°C by a measurement method based on JIS K6767.

[0159] <Interlaminar strength>

[0160] Figure 1 A schematic diagram of a test apparatus for evaluating interlaminar strength is shown in the figure. After applying a primer (manufactured by Semidyne Co., Ltd., "PPX Primer") to a 25 mm square range on the foam sheet 11, a 5 mm diameter amount of adhesive 12 (manufactured by Semidyne Co., Ltd., "PPX") is dripped in the center of the coated portion. Then, a 25 mm square aluminum clamp 13 is immediately placed on the adhesive dripping portion, and the foam sheet and the clamp 13 are crimped. Then, the foam sheet is cut along the size of the clamp 13. Primer is applied to the surface of the cut foam sheet to which the clamp 13 is not bonded, and a 5 mm diameter amount of adhesive 12 is dripped in the center of the coated portion. Then, a 10 mm square aluminum clamp 14 is immediately placed on the adhesive dripping portion, and the foam sheet and the clamp 14 are crimped. After wiping off the adhesive that has overflowed around the jig 14, a cut 15 is formed in the foam sheet along the size of the jig 14. The sheet is left at room temperature for 30 minutes to cure the adhesive, thereby preparing a sample for measuring interlayer strength.

[0161] Next, a 1 kN load cell is set in a testing machine (manufactured by A&D Co., Ltd., "Tensilon Universal Material Testing Machine") that is equipped with a thermostatic bath in such a way that tests can be performed in the thermostatic bath. Then, the sample for measuring interlayer strength is mounted on the testing machine in such a way that the sheet surface of the foam sheet is perpendicular to the stretching direction. After setting the temperature of the thermostatic bath to 23°C, leave it until the temperature of the sample for measuring interlayer strength reaches 23°C. Then, stretch one side of the clamp vertically upward at a speed of 100 mm / min to peel off only a 1 cm square area on the foam sheet. Measure the maximum load at this time as the first measurement result. Repeat the same operation three times, and take the average value as the interlayer strength.

[0162] <Stress Relaxation Rate>

[0163] The foam sheet was cut into a flat square of 10 mm × 10 mm, laminated to a thickness of 4 mm to make a test piece, and a tensile tester (made by Shimadzu Corporation, Autograph AGS-X) was used to compress the test piece to a stress A of 1.2 MPa at a speed of 5 mm / min, and the test piece was kept still for 1 minute in this state. The value B of the stress that becomes the lowest in a static state is measured, and the stress relaxation rate is calculated by the following formula. It should be noted that the measurement was carried out under an environment of 23°C and 50% RH.

[0164] Stress relaxation rate (%) = (AB) / A×100

[0165] <Closed Porosity>

[0166] A flat square test piece with a side of 5 cm was cut from the foam sheet. Then, the thickness of the test piece was measured, the apparent volume V1 of the test piece was calculated, and the mass W1 of the test piece was measured. Next, the volume V2 occupied by the bubbles was calculated based on the following formula. It should be noted that the density of the test piece is designated as ρ (g / cm 3 ).

[0167] The volume occupied by the bubble V2 = V1-W1 / ρ

[0168] Next, the test piece was immersed in 23°C distilled water at a depth of 100 mm from the water surface, and a pressure of 15 kPa was applied to the test piece for 3 minutes. Then, the test piece was taken out of the water, the water attached to the surface of the test piece was removed, the mass W2 of the test piece was measured, and the closed porosity F1 was calculated based on the following formula.

[0169] Closed-cell rate F1 (%) = 100-100 × (W2-W1) / V2

[0170] <Gel fraction>

[0171] A test piece of about 100 mg was collected from the foam sheet, and the mass C (mg) of the test piece was accurately weighed. Next, the test piece was immersed in 120°C xylene for 30 cm 3 After being left in the water for 24 hours, the mixture was filtered through a 200-mesh metal mesh, the insoluble components on the metal mesh were collected, vacuum dried, and the mass D (mg) of the insoluble components was accurately weighed. The gel fraction (mass %) was calculated from the obtained value by the following formula.

[0172] Gel fraction (mass %) = 100 × (D / C)

[0173] <Evaluation of permanent deformation>

[0174] The foam sheet is cut into a flat square of 10mm×10mm, stacked to a thickness of about 4mm, and a test piece is made to measure the thickness (E) of the test piece. Using a tensile testing machine (manufactured by Shimadzu Corporation, Autograph AGS-X), the test piece is compressed to a stress of 1.2MPa at a speed of 5mm / min, and is kept still for 1 minute in this state. Then, the compression is released and the thickness (F) of the test piece after compression is measured. Then, the permanent deformation rate is calculated by the following formula. Then, it is evaluated as follows. It should be noted that the determination of the permanent deformation rate is carried out under an environment of 23°C and 50%RH.

[0175] Permanent deformation rate (%) = (1-F / E) × 100 (Evaluation standard)

[0176] ○: Permanent deformation rate is 16% or more

[0177] △: Permanent deformation rate is 15%

[0178] ×: Permanent deformation rate is less than 15%

[0179] The materials used in Examples and Comparative Examples are as follows.

[0180] Elastomer resin (a): EP1001 (manufactured by Mitsui Chemicals, Inc., 4-methyl-1-pentene / propylene copolymer)

[0181] Elastomer resin (b): EP1013 (Mitsui Chemicals, Inc., 4-methyl-1-pentene / propylene copolymer)

[0182] Elastomer resin (c): SOE (registered trademark) S1605 (manufactured by Asahi Kasei Corporation, hydrogenated styrene-based thermoplastic elastomer (SEBS))

[0183] Elastomer resin (d): HIBLAR (registered trademark) 5127 (manufactured by KURARAY CO., LTD., styrene-based thermoplastic elastomer (SIS))

[0184] Polyolefin resin (a): KANEL (registered trademark) KF283 (manufactured by Japan Polyethylene Co., Ltd., ethylene / α-olefin copolymer (LLDPE) polymerized using a metallocene catalyst)

[0185] Thermal decomposition type foaming agent: azodicarbonamide

[0186] Decomposition temperature regulator: zinc oxide, manufactured by Sakai Chemical Industry Co., Ltd., trade name "OW-212F"

[0187] Phenolic antioxidant: 2,6-di-tert-butyl-p-cresol

[0188] [Method for producing foam sheet]

[0189] The foamed sheets of Examples 1 to 12 and Comparative Examples 1 and 2 were produced as follows.

[0190] <Example 1>

[0191] Prepare 50 parts by mass of elastomer resin (a), 50 parts by mass of polyolefin resin (a), 3 parts by mass of thermal decomposition type foaming agent, 1 part by mass of decomposition temperature regulator, and 0.5 parts by mass of phenolic antioxidant as raw materials. After melt-kneading these materials, a foamable resin sheet with a thickness of 0.15 mm is obtained by pressing. Both sides of the obtained foamable resin sheet are irradiated with 6.5 Mrad of electron beam at an accelerating voltage of 500 keV to crosslink the foamable resin sheet. Next, the cross-linked foamable resin sheet is stretched along MD and TD in a manner to achieve the flatness recorded in Table 1, while being heated to 250°C, thereby causing it to foam and obtain a density of 0.51 g / cm 3 , foam sheet with a thickness of 0.10mm.

[0192] <Example 2>

[0193] The foam sheet was obtained in the same manner as in Example 1, except that the amount of the elastomer resin (a) was changed from 50 parts by mass to 30 parts by mass, the amount of the polyolefin resin (a) was changed from 50 parts by mass to 70 parts by mass, and the sheet was stretched in MD and TD in such a manner as to achieve the flatness described in Table 1.

[0194] <Example 3>

[0195] The amount of the elastomer resin (a) was changed from 50 parts by mass to 30 parts by mass, the amount of the polyolefin resin (a) was changed from 50 parts by mass to 70 parts by mass, and the amount of the thermal decomposition type foaming agent was changed from 3 parts by mass to 4.2 parts by mass. The irradiation amount of the electron beam was changed from 6.5 Mrad to 6 Mrad, and the foamable resin sheet was stretched in MD and TD so as to achieve the flatness described in Table 1. Except for this, the same operation as in Example 1 was performed to obtain a foamed sheet.

[0196] <Example 4>

[0197] The elastomer resin (a) was changed to the elastomer resin (b), the amount of the thermal decomposition type foaming agent was changed from 3 parts by mass to 5.5 parts by mass, the irradiation amount of the electron beam was changed from 6.5 Mrad to 6 Mrad, and the sheet was stretched in MD and TD in such a manner as to achieve the flatness described in Table 1. The same operations as in Example 1 were performed to obtain a foam sheet.

[0198] <Example 5>

[0199] The elastomer resin (a) was changed to the elastomer resin (b), the amount of the thermal decomposition type foaming agent was changed from 3 parts by mass to 4.5 parts by mass, the irradiation amount of the electron beam was changed from 6.5 Mrad to 8 Mrad, and the sheet was stretched in MD and TD in a manner to achieve the flatness described in Table 1. The same operations as in Example 1 were performed to obtain a foam sheet.

[0200] <Example 6>

[0201] The elastomer resin (a) was changed to the elastomer resin (c), the amount of the thermal decomposition type foaming agent was changed from 3 parts by mass to 5 parts by mass, the irradiation amount of the electron beam was changed from 6.5 Mrad to 6 Mrad, and the sheet was stretched in MD and TD in such a manner as to achieve the flatness described in Table 1. The same operations as in Example 1 were performed to obtain a foam sheet.

[0202] <Example 7>

[0203] A foam sheet was obtained by performing the same operations as in Example 6, except that the amount of the elastomer resin (c) was changed from 50 parts by mass to 60 parts by mass, the amount of the polyolefin resin (a) was changed from 50 parts by mass to 40 parts by mass, and the amount of electron beam irradiation was changed from 6 Mrad to 8 Mrad.

[0204] <Example 8>

[0205] The foam sheet was obtained in the same manner as in Example 6, except that the amount of elastomer resin (c) was changed from 50 parts by mass to 90 parts by mass, the amount of polyolefin resin (a) was changed from 50 parts by mass to 10 parts by mass, the amount of thermal decomposition type foaming agent was changed from 5 parts by mass to 4 parts by mass, and the acceleration voltage was changed from 500 keV to 1000 keV.

[0206] <Example 9>

[0207] The elastomer resin (a) was changed to the elastomer resin (d), the amount of the thermal decomposition type foaming agent was changed from 3 parts by mass to 5 parts by mass, the irradiation amount of the electron beam was changed from 6.5 Mrad to 6 Mrad, and the sheet was stretched along MD and TD in such a manner as to achieve the flatness described in Table 1. A foam sheet was obtained in the same manner as in Example 1.

[0208] <Example 10>

[0209] The amount of the elastomer resin (a) was changed from 50 parts by mass to 25 parts by mass, the amount of the polyolefin resin (a) was changed from 50 parts by mass to 75 parts by mass, and the amount of the thermal decomposition type foaming agent was changed from 3 parts by mass to 5 parts by mass. The irradiation amount of the electron beam was changed from 6.5 Mrad to 7 Mrad, and the foamable resin sheet was stretched in MD and TD so as to achieve the flatness described in Table 1. Except for this, the same operation as in Example 1 was performed to obtain a foamed sheet.

[0210] <Example 11>

[0211] The elastomer resin (a) was changed to the elastomer resin (b), the blending amount was changed from 50 parts by mass to 40 parts by mass, the blending amount of the polyolefin resin (a) was changed from 50 parts by mass to 60 parts by mass, and the blending amount of the thermal decomposition type foaming agent was changed from 3 parts by mass to 4.5 parts by mass. In addition, the irradiation amount of the electron beam was changed from 6.5 Mrad to 7 Mrad, and the sheet was stretched in MD and TD in such a manner as to achieve the flattening ratio described in Table 1. Except for this, the same operation as in Example 1 was performed to obtain a foam sheet.

[0212] <Example 12>

[0213] The elastomer resin (a) was changed to the elastomer resin (c), the blending amount was changed from 50 parts by mass to 40 parts by mass, the blending amount of the polyolefin resin (a) was changed from 50 parts by mass to 60 parts by mass, and the blending amount of the thermal decomposition type foaming agent was changed from 3 parts by mass to 5.4 parts by mass. The irradiation amount of the electron beam was changed from 6.5 Mrad to 7 Mrad, and the sheet was stretched in MD and TD so as to achieve the flatness described in Table 1. Except for this, the same operation as in Example 1 was performed to obtain a foam sheet.

[0214] <Comparative Example 1>

[0215] The same operations as in Example 1 were performed except that the amount of the elastomer resin (a) was changed from 50 parts by mass to 0 parts by mass, the amount of the polyolefin resin (a) was changed from 50 parts by mass to 100 parts by mass, the amount of electron beam irradiation was changed from 6.5 Mrad to 6 Mrad, and the film was stretched in MD and TD in such a manner as to achieve the flatness described in Table 1, thereby obtaining a foam sheet.

[0216] <Comparative Example 2>

[0217] The same operations as in Example 9 were performed except that the amount of elastomer resin (d) was changed from 50 parts by mass to 10 parts by mass, the amount of polyolefin resin (a) was changed from 50 parts by mass to 90 parts by mass, the amount of electron beam irradiation was changed from 6.5 Mrad to 7 Mrad, and the film was stretched along MD and TD in a manner to achieve the flatness described in Table 1.

[0218] Table 1 shows the evaluation results of Examples 1 to 12 and Comparative Examples 1 and 2.

[0219]

[0220] From the evaluation results of the foam sheets of Examples 1 to 12 and Comparative Examples 1 to 2, it can be seen that when the stress relaxation rate is 23% or more and the 25% compressive strength is 1000 kPa or less, the permanent deformation of the foam sheet becomes larger. It can be seen that by using the foam sheets of Examples 1 to 12 for adhesive tapes, when the adhesive tapes are attached to a curved surface to fix a component, it is possible to suppress the problem of the fixed component floating due to the deviation of the curved surface tolerance.

[0221] Explanation of symbols

[0222] 1 Drawing

[0223] 2 Foam Strips

[0224] 3 Housing

[0225] 11 Foam sheet

[0226] 12 Adhesive

[0227] 13. Fixture

[0228] 14. Fixture

[0229] 15. Incision

Claims

1. A foam sheet having a stress relaxation rate of 23% or more and a 25% compression strength of 1000 kPa or less.

2. The foam sheet according to claim 1, which has an interlaminar strength of 0.6 MPa or more.

3. The foam sheet according to claim 1 or 2, which has a closed cell ratio of 80% or more. 4 . The foam sheet according to claim 1 , which has a gel fraction of 30 to 80%. 5 . The foam sheet according to claim 1 , wherein the larger of the MD flatness and the TD flatness of the cells is 2 or more.

6. The foam sheet according to any one of claims 1 to 5, which has a density of 0.05 to 0.6 g / cm 3 .

7. The foam sheet according to any one of claims 1 to 6, which has a thickness of 0.03 to 2 mm. 8 . The foam sheet according to claim 1 , wherein the foam sheet has at least one temperature showing a maximum value of the loss tangent tan δ of dynamic viscoelasticity within a range of 15 to 50° C. 9 . The foam sheet according to claim 1 , wherein the maximum value of the loss tangent tan δ of the dynamic viscoelasticity is 0.2 or more. 10 . A pressure-sensitive adhesive tape comprising the foam sheet according to claim 1 , and a pressure-sensitive adhesive material provided on at least one surface of the foam sheet.