Non-quenched and tempered steel wire for hot forging with improved workability and toughness and method for manufacturing same

By forming TiN and AlN in non-tempered steel and adding Ca, the problem of insufficient toughness of non-tempered steel is solved, and high toughness and processability under no heat treatment conditions are achieved. It is suitable for automobiles or mechanical components. Reduced costs and environmental impacts.

CN119013428APending Publication Date: 2024-11-22POHANG IRON & STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380034024.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-05-27
Filing Date
2023-05-26
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The toughness of non-temperature steel is poor, making it difficult to meet the demands of automotive or mechanical components for machiningability and impact toughness without heat treatment, and traditional methods can lead to reduced toughness when improving machiningability by adding MnS.

Method used

The grain size is reduced by adding TiN and AlN in non-tempered steel, and suppressing the elongation of MnS by the addition of Ca, forming Ca-based oxides to improve processability and toughness, satisfying specific chemical composition and heat treatment condition.

Benefits of technology

It realizes the processability and impact toughness of non-temperature steel without heat treatment, making it suitable for automotive or mechanical components that require high toughness and machining, reducing production costs and environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005082814190000091
    Figure BDA0005082814190000091
  • Figure BDA0005082814190000092
    Figure BDA0005082814190000092
  • Figure BDA0005082814190000101
    Figure BDA0005082814190000101
Patent Text Reader

Abstract

A non-quenched and tempered steel wire for hot forging having improved workability and toughness and a method for manufacturing the same are disclosed. The non-quenched and tempered steel wire rod according to the present invention contains, in wt%, C: 0.3% to 0.5%, Si: 0.4% to 0.9%, Mn: 0.5% to 1.2%, P: 0.02% or less, S: 0.01% to 0.05%, soluble Al: 0.01% to 0.05%, Cr: 0.1% to 0.3%, Ti: 0.01% to 0.02%, Ca: 0.0005% to 0.002%, and N: 0.007% to 0.02%, the remainder being Fe and unavoidable impurities, and further contains ferrite and pearlite as a microstructure, and satisfies relational expression 1. [relational expression 1] 2 < = (Al + Ti) / N < = 5.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a non-quenched and tempered steel wire having improved workability and impact toughness and a method for manufacturing the same, and more particularly, to a non-quenched and tempered steel wire suitable for use as a material for automobile or mechanical parts and a method for manufacturing the same. Background Art

[0002] Unlike quenched and tempered steel that obtains a certain level of strength and toughness through quenching and tempering (QT) heat treatment, the QT heat treatment process is omitted in non-quenched and tempered steel. Therefore, non-quenched and tempered steel is economically advantageous not only by reducing heat treatment costs, simplifying processes to shorten delivery time, and improving productivity, but also by reducing CO generated by operating a furnace during heat treatment. 2 It is environmentally friendly. At the beginning of development, since the toughness of non-quenched and tempered steel is inferior to that of quenched and tempered steel, non-quenched and tempered steel is only applied to parts that do not require high toughness. However, with the recent increase in demand for environmental feasibility and cost reduction, the demand for improving the toughness of non-quenched and tempered steel is increasing. In addition, since the cutting process is often performed to obtain the final shape of the component, machinability is also required. Generally, a large amount of MnS is generated by adding S to improve machinability, resulting in a problem of reduced toughness of the product. Summary of the invention

[0003] Technical issues

[0004] The present disclosure provides a non-quenched and tempered steel wire rod having a disadvantage of being inferior to conventional quenched and tempered steel in toughness and having both impact toughness and workability by reducing the grain size through the formation of TiN and AlN and suppressing the elongation of MnS through the addition of Ca without additional heat treatment, and a method for manufacturing the same.

[0005] Technical Solution

[0006] A non-quenched and tempered steel wire rod with improved workability and impact toughness according to one embodiment of the present disclosure contains, in terms of weight percentage (wt%), 0.3% to 0.5% C, 0.4% to 0.9% Si, 0.5% to 1.2% Mn, 0.02% or less P, 0.01% to 0.05% S, 0.01% to 0.05% soluble Al, 0.1% to 0.3% Cr, 0.01% to 0.02% Ti, 0.0005% to 0.002% Ca, 0.007% to 0.02% N, and the remainder being Fe and unavoidable impurities, further contains ferrite and pearlite as microstructures, and satisfies the following relational expression 1.

[0007] [Relational Expression 1]2≤(Al+Ti) / N≤5

[0008] A method for manufacturing a non-quenched and tempered steel wire having improved workability and impact toughness according to an embodiment of the present disclosure comprises: reheating a steel piece at a temperature ranging from 950° C. to 1120° C., wherein the steel piece comprises, in terms of weight percentage (wt%): 0.3% to 0.5% C, 0.4% to 0.9% Si, 0.5% to 1.2% Mn, 0.02% or less P, 0.01% to 0.05% S, 0.01% to 0. 05% to 0.05% of soluble Al, 0.1% to 0.3% of Cr, 0.01% to 0.02% of Ti, 0.0005% to 0.002% of Ca, 0.007% to 0.02% of N, and the remainder being Fe and inevitable impurities; finish rolling the reheated steel piece into a steel wire rod at a temperature of 750° C. to 850° C.; and coiling the steel wire rod and cooling the steel wire rod to 400° C. at an average cooling rate range of 0.1° C. / sec to 5.0° C. / sec.

[0009] Beneficial Effects

[0010] In the non-quenched and tempered steel wire rod with improved workability and impact toughness according to one embodiment of the present disclosure, Ti and Al are combined with N to form nitrides such as TiN and AlN, and such nitrides interfere with the growth of grain boundaries to reduce the grain size, thereby improving toughness. In addition, Ca-based oxides generated by the addition of Ca serve as nuclei for the formation of MnS and suppress the elongation of MnS during rolling to improve workability and toughness. Therefore, even if heat treatment is omitted, the steel wire rod can be applied to materials used in automobiles or mechanical parts that require both workability and toughness. DETAILED DESCRIPTION

[0011] A non-quenched and tempered steel wire rod with improved workability and impact toughness according to one embodiment of the present disclosure contains, in terms of weight percentage (wt%), 0.3% to 0.5% C, 0.4% to 0.9% Si, 0.5% to 1.2% Mn, 0.02% or less P, 0.01% to 0.05% S, 0.01% to 0.05% soluble Al, 0.1% to 0.3% Cr, 0.01% to 0.02% Ti, 0.0005% to 0.002% Ca, 0.007% to 0.02% N, and the remainder being Fe and unavoidable impurities, further contains ferrite and pearlite as microstructures, and satisfies the following relational expression 1.

[0012] [Relational Expression 1]2≤(Al+Ti) / N≤5

[0013] Embodiments of the invention

[0014] This specification does not describe all the elements of the embodiments of the present disclosure, and a detailed description of content known in the art or a redundant description of substantially the same configuration can be omitted. In addition, unless otherwise specified, the term "comprising" an element does not exclude other elements, but may also include other elements. As used herein, unless the context clearly indicates otherwise, the singular form is intended to also include the plural form. Hereinafter, the present disclosure will be described in detail.

[0015] The present inventors have examined methods for providing a steel wire having both workability and impact toughness from various viewpoints, and have found that workability and toughness can be obtained by appropriately controlling the composition of alloy elements and the microstructure of the steel wire without separate heat treatment, thereby completing the present disclosure.

[0016] A non-quenched and tempered steel wire rod with improved workability and impact toughness according to one embodiment of the present disclosure contains, in terms of weight percentage (wt%), 0.3% to 0.5% C, 0.4% to 0.9% Si, 0.5% to 1.2% Mn, 0.02% or less P, 0.01% to 0.05% S, 0.01% to 0.05% soluble Al, 0.1% to 0.3% Cr, 0.01% to 0.02% Ti, 0.0005% to 0.002% Ca, 0.007% to 0.02% N, and the remainder being Fe and unavoidable impurities, and satisfies the following relational expression 1.

[0017] [Relational Expression 1]2≤(Al+Ti) / N≤5

[0018] Hereinafter, the reason for numerically limiting the content of alloy elements in the embodiment of the present disclosure will be described. Hereinafter, unless otherwise specified, the unit is weight %.

[0019] The C content is 0.3% to 0.5%.

[0020] Carbon (C) is an element for improving the strength of the steel wire rod. In order to obtain the above-mentioned effect, C is preferably contained in an amount of 0.3% or more. However, an excessive C content may deteriorate toughness and workability, and thus the upper limit of the C content may be controlled to 0.5%.

[0021] The content of Si is 0.4% to 0.9%.

[0022] Silicon (Si) is an element effective as a deoxidizer and is used to improve strength. When the Si content is less than 0.4%, the above effect cannot be obtained. When the Si content exceeds 0.9%, the deformation resistance of the steel increases rapidly due to solid solution strengthening. Therefore, the upper limit of the Si content can be controlled to 0.9%.

[0023] The content of Mn is 0.5% to 1.2%.

[0024] Manganese (Mn) is an element effective as a deoxidizer and desulfurizer. When the Mn content is less than 0.5%, the above effects cannot be obtained. When the Mn content exceeds 1.2%, the strength of the steel increases excessively, so that the deformation resistance of the steel increases rapidly, resulting in deterioration of cold workability. Therefore, the upper limit of the Mn content can be controlled to 1.2%.

[0025] The content of Cr is 0.1% to 0.3%.

[0026] Chromium (Cr) is an element for promoting the transformation of ferrite and pearlite during hot rolling. In addition, Cr does not increase the strength of steel too much, reduces the amount of solid solution of C by precipitating carbides, and helps to reduce dynamic strain aging caused by solid solution of carbon. In the case where the Cr content is less than 0.1%, the above effect cannot be obtained, and in the case where the Cr content exceeds 0.3%, the strength of the steel is excessively increased, so that the deformation resistance of the steel increases rapidly, resulting in deterioration of cold workability. Therefore, the upper limit of the Cr content can be controlled to 0.3%.

[0027] The content of P is 0.02% or less.

[0028] Phosphorus (P), as an impurity inevitably contained in steel, is a main causative element that segregates into grain boundaries, causing toughness degradation and delayed fracture resistance reduction. Therefore, it is preferable to control the P content as low as possible. Theoretically, it is preferable to control the P content to 0%, but P is inevitably contained therein during the manufacturing process. Therefore, it is important to control the upper limit, and in the present disclosure, the upper limit of the P content can be controlled to 0.02%.

[0029] The content of S is 0.01% to 0.05%.

[0030] Sulfur (S) is an impurity inevitably contained in steel during the manufacturing process as a main causative element that segregates into grain boundaries and causes significant deterioration of ductility in steel and formation of sulfide inclusions, thereby causing deterioration of delayed fracture resistance and stress relaxation. However, as in the present disclosure, S can be actively used to improve workability. Since S combines with Mn to form MnS that improves workability, in consideration of the S content that is effective for improving workability without significantly impairing the toughness of the steel, the S content is controlled within a range of 0.01% to 0.05% in the present disclosure.

[0031] The content of soluble Al is 0.01% to 0.05%.

[0032] Soluble Al is an element effective as a deoxidizer. Soluble Al may be included in an amount of 0.01% to obtain the above-mentioned effect. However, in the case where the Al content exceeds 0.05%, difficulties may occur during the casting process due to Al oxides. Therefore, the upper limit of the Al content may be controlled to 0.05% in the present disclosure.

[0033] The content of Ti is 0.01% to 0.02%.

[0034] Titanium (Ti) is an element that plays a major role in improving the toughness of steel by forming TiN precipitates during the solidification process of steel to suppress the growth of austenite grains during the heating and hot rolling processes of the slab to reduce the grain size of the final structure. In the case where the Ti content is less than 0.01%, it is difficult to obtain a sufficient amount of TiN precipitates to suppress the migration of austenite grain boundaries. On the contrary, in the case where the Ti content exceeds 0.02%, coarse titanium nitride may be formed, which deteriorates the toughness, and therefore the upper limit of the Ti content may be controlled to 0.02% in the present disclosure.

[0035] The content of Ca is 0.0005% to 0.002%.

[0036] Ca is an essential element for achieving the effect of improving machinability and impact toughness by reducing the aspect ratio of MnS. The addition of Ca leads to the formation of oxides that act as the core of MnS to suppress the elongation of MnS while rolling the steel wire and maintain a low aspect ratio. The low aspect ratio of MnS not only improves machinability, but also suppresses the deterioration of toughness by reducing the anisotropy of the microstructure. However, Ca should be added in an amount of 0.0005% or more to obtain the above-mentioned effect, but a Ca content exceeding 0.002% may cause difficulties in the manufacturing process. Therefore, the upper limit of the Ca content is controlled to 0.002%.

[0037] The content of N is 0.007% to 0.02%.

[0038] N is an essential element for achieving the effect of improving impact toughness by reducing the grain size through the formation of nitrides with Ti and Al. When the N content is less than 0.007%, it is difficult to obtain a sufficient amount of nitrides, resulting in a reduction in the generation of precipitates of Al, Ti, etc., and the toughness desired in the present disclosure cannot be obtained. When the N content exceeds 0.02%, the solid solution of N that does not exist as a nitride increases to deteriorate the toughness and ductility of the steel wire. Therefore, in the present disclosure, the upper limit of the N content can be controlled to 0.02%.

[0039] The remaining component of the non-quenched and tempered steel wire of the present disclosure is iron (Fe). However, the non-quenched and tempered steel wire may contain other impurities incorporated during the common industrial manufacturing process of steel. Impurities are not specifically mentioned in the present disclosure because they are known to any person skilled in the art of manufacturing.

[0040] The non-quenched and tempered steel wire rod according to one embodiment of the present disclosure may satisfy relational expressions 1 to 3.

[0041] In relational expressions 1 to 3, [Al], [Ti], [N], [S], [Ca], [C], [Si], and [Mn] respectively represent elements and their contents (weight %).

[0042] [Relational Expression 1]2≤([Al]+[Ti]) / [N]≤5(toughness)

[0043] Relational expression 1 is an expression related to toughness. According to the present disclosure, TiN and AlN are formed by adding high contents of N, Ti and Al. Since the precipitation of fine TiN and AlN in the steel inhibits the growth of grains, the grains are refined to improve the impact toughness of the non-quenched and tempered steel wire according to the present disclosure. It is preferred to form as many TiN and AlN precipitates as possible with a size of about 50 nm to obtain the above-mentioned effect, and for this purpose, it is necessary to control the ([Al] + [Ti]) / [N] ratio within the range of 2 to 5. At a ([Al] + [Ti]) / [N] ratio of less than 2, precipitates cannot be fully formed. At a ([Al] + [Ti]) / [N] ratio exceeding 5, the formation of coarse precipitates may be caused, which in turn leads to deterioration of toughness. Therefore, according to the present disclosure, the ([Al] + [Ti]) / [N] ratio is controlled within the range of 2 to 5.

[0044] [Relational Expression 2] 10≤[S] / [Ca]≤70 (processability and impact toughness)

[0045] Relational expression 2 is an expression related to machinability and impact toughness. According to the present disclosure, MnS is formed by adding a high S content. MnS, as an elongated inclusion, has a shape and orientation that is elongated in the rolling direction, and significantly improves the machinability of the non-quenched and tempered steel wire rod of the present disclosure. However, in the case of applying an impact thereto, MnS acts as the starting point of the crack and its propagation path, thereby deteriorating the impact toughness. Therefore, Ca is added to suppress the elongation of MnS, and for this reason, the S / Ca ratio is preferably controlled within a range of 10 to 70. At an S / Ca ratio of less than 10, it is difficult to obtain the desired machinability in the present disclosure because the content of S is insufficient relative to the content of Ca. On the contrary, at an S / Ca ratio of more than 70, the elongation of MnS cannot be effectively suppressed because a sufficient amount of Ca oxide capable of suppressing the elongation of MnS is not obtained, making it difficult to obtain toughness. Therefore, in the present disclosure, the S / Ca ratio is controlled within a range of 10 to 70 to obtain a combination of excellent machinability and impact toughness.

[0046] [Relational Expression 3] 700≤300+903X[C]+95X[Si]+154X[Mn]-2303X[S](strength)

[0047] Relational expression 3 is an expression related to strength. C, Si and Mn are elements having a large solid solution strengthening effect. On the contrary, since S forms MnS to reduce the amount of Mn effective for promoting solid solution strengthening, the strength decreases. Therefore, it is necessary to control the value of relational expression 3 to 700 or more in order to obtain a strength of the steel wire of 700 MPa or more.

[0048] The non-quenched and tempered steel wire according to one embodiment of the present disclosure includes ferrite and pearlite as microstructures, and an average interlaminar spacing between ferrite and pearlite may be 10.0 μm to 15.0 μm, preferably 12.0 μm to 13.0 μm.

[0049] In addition, the thickness of ferrite of the non-quenched and tempered steel wire according to one embodiment of the present disclosure may be 5.0 μm to 10.0 μm, preferably 7.0 μm to 9.0 μm.

[0050] Furthermore, the aspect ratio of ferrite of the non-quenched and tempered steel wire rod according to one embodiment of the present disclosure may be 4 or less.

[0051] In addition, the tensile strength of the non-quenched and tempered steel wire according to one embodiment of the present disclosure may be 700 MPa or more.

[0052] In addition, the non-quenched and tempered steel wire according to one embodiment of the present disclosure may have a yield strength of 350 MPa to 450 MPa.

[0053] In addition, the non-quenched and tempered steel wire rod according to one embodiment of the present disclosure may have a yield ratio of 0.45 to 0.65.

[0054] In addition, the impact toughness of the non-quenched and tempered steel wire according to one embodiment of the present disclosure may be 60 J / cm 2 or larger.

[0055] In addition, the product of the tensile strength and impact toughness of the non-quenched and tempered steel wire according to one embodiment of the present disclosure may be 30,000 to 60,000.

[0056] Hereinafter, a method for manufacturing a non-quenched and tempered steel wire rod according to one embodiment of the present disclosure will be described.

[0057] The non-quenched and tempered steel wire having improved workability and impact toughness according to the present disclosure may be manufactured by using various methods, and the method is not particularly limited. However, according to one embodiment, the steel wire may be manufactured by using the following method.

[0058] A method for manufacturing a non-quenched and tempered steel wire rod having improved workability and impact toughness according to the present disclosure includes: reheating a steel piece, the steel piece comprising, in weight percentage (wt%): 0.3% to 0.5% C, 0.4% to 0.9% Si, 0.5% to 1.2% Mn, 0.02% or less P, 0.01% to 0.05% S, 0.01% to 0.05% soluble Al, 0.1% to 0.3% Cr, 0.01% to 0.02% Ti, 0.0005% to 0.002% Ca, 0.007% to 0.02% N, and the remainder being Fe and unavoidable impurities, and further comprising ferrite and pearlite as microstructures; hot rolling the reheated steel piece into a steel wire rod; and coiling and cooling the steel wire rod.

[0059] Hereinafter, each process of the manufacturing method will be described in more detail.

[0060] First, a billet satisfying the composition of the above-mentioned alloy elements is heated and rolled into a steel billet.

[0061] Reheating process

[0062] As a step of reheating the rolled steel billet, the reheating process is a process for reducing the rolling load when rolling the steel wire rod. In this regard, the reheating can be performed at a temperature of 950°C to 1,120°C. At a reheating temperature below 950°C, the rolling load may increase, causing difficulties in the manufacturing method. On the contrary, at a reheating temperature above 1,120°C, all of the AlN finely formed in the steel piece may form a solid solution again during heating, thereby significantly reducing the grain refinement effect.

[0063] The process of rolling steel wire

[0064] In the process of rolling the steel wire rod, the reheated steel piece is hot rolled into the steel wire rod.

[0065] In this case, the finishing temperature of hot rolling may be 750 to 850° C. At a finishing temperature below 750° C., rolling load may increase, while at a finishing temperature above 850° C., grains may coarsen, so that high toughness desired in the present disclosure may not be obtained.

[0066] Winding process

[0067] A process of winding the steel wire manufactured as described above into the shape of a coil may be performed. In this case, the coiling temperature may be 750°C to 850°C. Since the temperature of the steel wire obtained by finish rolling may be increased by transformation heating, the temperature of the steel wire immediately before coiling may be higher than the finish rolling temperature. In this case, the steel wire may be coiled after being cooled to the coiling temperature, or may be coiled without a separate cooling process according to the temperature increased by heating. At a coiling temperature below 750°C, the martensite generated in the surface layer during cooling cannot be recovered due to residual heat, and tempered martensite is formed, causing a problem of increasing the possibility of inducing surface defects during the drawing process. On the contrary, at a coiling temperature above 850°C, a thick scale may be formed on the surface of the steel wire, so that surface defects may easily occur during descaling, and productivity may be deteriorated due to an increase in cooling time in the subsequent cooling process.

[0068] Cooling process

[0069] The coiled steel wire may be cooled, and in this case, the cooling process may be performed to 400° C. by air cooling or controlled cooling in an average cooling rate range of 0.1° C. / sec to 5.0° C. / sec after hot forging. At an average cooling rate lower than 0.1° C. / sec when cooling to 400° C. after coiling, the desired strength cannot be obtained due to excessive formation of proeutectoid ferrite. At an average cooling rate higher than 5° C. / sec, a low-temperature structure such as martensite may be generated, and thus toughness and workability may be deteriorated.

[0070] {Example}

[0071] A square billet having a composition of alloy elements shown in Table 1 was heated at 1,200°C for 4 hours and rolled into a steel billet at a finishing temperature of 1,100°C. Then, the steel billet was heated at 1,090°C for 90 minutes, finish rolled at 800°C, coiled at 780°C, and cooled into a steel wire having a diameter of 26 mm. Steel wires (Table 1) containing the components of Inventive Steels 1 to 7 and Comparative Steels 1 to 4 were manufactured, and the tensile strength and impact toughness of the samples of the steel wires were measured and are shown in Table 2 below.

[0072] Here, the room temperature tensile strength is measured at 25°C at the center of a sample of non-quenched and tempered steel, and the room temperature impact toughness is measured at 25°C at a sample with a U-shaped notch (based on a standard sample, 10 mm×10 mm×55 mm) using the Charpy impact energy value obtained by a Charpy impact test.

[0073] In addition, in order to evaluate the machinability, a steel wire rod having a diameter of 26 mm was processed into a cold drawn bar (CD bar) having a diameter of 24 mm at a reduction rate of 14.8%. The machinability was evaluated by using a CNC lathe, and the breaking of the turning chips was evaluated after the turning operation was performed until the CD bar having a diameter of 24 mm was reduced to a diameter of 15 mm. In this case, cutting was performed under the conditions of a cutting rate of 100 mm / min, a feed rate of 0.1 mm / rev, and a cutting depth of 1.0 mm by using cutting oil. The breaking of the chips was evaluated based on the number of turns of chips generated during the turning process, and 5 or less chips were evaluated as good, more than 5 but not more than 10 chips were evaluated as fair, and more than 10 chips were evaluated as poor.

[0074] [Table 1]

[0075]

[0076] [Table 2]

[0077]

[0078]

[0079] As shown in Tables 1 and 2, the steel wires of Examples 1 to 7 satisfying all of the chemical compositions, relational expressions, and manufacturing conditions provided in the present disclosure have a tensile strength of 700 MPa or more, a strength of 60 J / cm 2or greater impact toughness and good workability. On the contrary, it was determined that the steel wires of Comparative Examples 1 to 7 that did not satisfy at least one of the above conditions had one or more poor characteristics in tensile strength, workability and impact toughness. Specifically, Comparative Example 1 having a low C content failed to satisfy the recommended tensile strength of 700 MPa or more, and Comparative Example 2 having an excessive Si and an S / Ca value of only 8 had poor workability. Comparative Example 3 that did not satisfy the recommended Mn content and Relational Expression 3 could not obtain sufficient strength. Comparative Example 4 that contained an excessive amount of Ti and did not satisfy Relational Expression 1 had insufficient toughness. Although Comparative Examples 5 to 7 satisfied the chemical composition suggested by the present disclosure, the heating temperature was outside the recommended range, or the average cooling rate was not satisfied when cooled to 400°C, and therefore the toughness and tensile strength were outside the target values.

[0080] While the present disclosure has been particularly described with reference to exemplary embodiments, it will be understood by those skilled in the art that various changes in form and details may be made therein without departing from the spirit and scope of the present disclosure.

[0081]

Industrial Applicability

[0082] According to the present disclosure, even when heat treatment is omitted, a non-quenched and tempered steel wire rod having both improved workability and toughness can be provided, and thus the present disclosure has industrial applicability.

Claims

1. A non-quenched and tempered steel wire rod having improved workability and impact toughness, comprising, in weight percentage (wt%): 0.3% to 0.5% C, 0.4% to 0.9% Si, 0.5% to 1.2% Mn, 0.02% or less P, 0.01% to 0.05% S, 0.01% to 0.05% soluble Al, 0.1% to 0.3% Cr, 0.01% to 0.02% Ti, 0.0005% to 0.002% Ca, 0.007% to 0.02% N, and the remainder being Fe and unavoidable impurities, and Contains ferrite and pearlite as microstructure, The steel wire rod satisfies the following relational expression 1: [Relational Expression 1]2≤(Al+Ti) / N≤5.

2. The non-quenched and tempered steel wire rod according to claim 1, wherein the non-quenched and tempered steel wire rod satisfies the following relational expression 2: [Relational Expression 2]10≤S / Ca≤70.

3. The non-quenched and tempered steel wire according to claim 1, wherein the non-quenched and tempered steel wire satisfies the following relational expression 3: [Relational Expression 3]700≤300+903X C+95X Si+154X Mn-2303X S.

4. The non-quenched and tempered steel wire rod according to claim 1, wherein an average interlayer spacing between ferrite and pearlite is 10.0 μm to 15.0 μm. 5 . The non-quenched and tempered steel wire rod according to claim 1 , wherein a thickness of the ferrite is 5.0 μm to 10.0 μm. 6 . The non-quenched and tempered steel wire rod according to claim 1 , wherein the aspect ratio of the ferrite is 4 or less.

7. The non-quenched and tempered steel wire rod according to claim 1, wherein the tensile strength is 700 MPa or more.

8. The non-quenched and tempered steel wire rod according to claim 1, wherein the yield strength is 350 MPa to 450 MPa.

9. The non-quenched and tempered steel wire rod according to claim 1, wherein the yield ratio is 0.45 to 0.

65.

10. The non-quenched and tempered steel wire according to claim 1, wherein the impact toughness is 60 J / cm 2 or larger.

11. The non-quenched and tempered steel wire rod according to claim 1, wherein the product of tensile strength and impact toughness is 30,000 to 60,000.

12. A method for producing a non-quenched and tempered steel wire having improved workability and impact toughness, the method comprising: reheating a steel article at a temperature in the range of 950° C. to 1120° C., the steel article comprising, in terms of weight percentage (wt%): 0.3% to 0.5% C, 0.4% to 0.9% Si, 0.5% to 1.2% Mn, 0.02% or less P, 0.01% to 0.05% S, 0.01% to 0.05% soluble Al, 0.1% to 0.3% Cr, 0.01% to 0.02% Ti, 0.0005% to 0.002% Ca, 0.007% to 0.02% N, and the remainder being Fe and inevitable impurities, and comprising ferrite and pearlite as a microstructure; Finish rolling the reheated steel piece into steel wire at a temperature of 750° C. to 850° C.; as well as The steel wire is coiled and cooled, The cooling performed after the coiling includes a process of cooling the steel wire to 400° C. at an average cooling rate of 0.1° C. / sec to 5.0° C. / sec, and the steel wire satisfies the following relational expression 1: [Relational Expression 1]2≤(Al+Ti) / N≤5.

13. The method according to claim 12, wherein the steel wire material satisfies the following relational expression 2: [Relational Expression 2]10≤S / Ca≤70.

14. The method according to claim 12, wherein the steel wire material satisfies the following relational expression 3: [Relational Expression 3]700≤300+903X C+95X Si+154X Mn-2303X S. 15 . The method according to claim 12 , wherein an average interlayer spacing between ferrite and pearlite of the steel wire rod is 10.0 μm to 15.0 μm. 16 . The method according to claim 12 , wherein the ferrite of the steel wire rod has a thickness of 5.0 μm to 10.0 μm. 17 . The method of claim 12 , wherein the ferrite of the steel wire rod has an aspect ratio of 4 or less.

18. The method of claim 12, wherein the steel wire has a tensile strength of 700 MPa or more.

19. The method of claim 12, wherein the steel wire has a yield strength of 350 MPa to 450 MPa.

20. The method of claim 12, wherein the steel wire has a yield ratio of 0.45 to 0.

65.

21. The method according to claim 12, wherein the impact toughness of the steel wire is 60 J / cm 2 or larger.