Method for preparing catalyst by using waste lithium ion battery and application of catalyst in hydrogen production
NiFeCoMnAl catalyst was prepared from the waste lithium-ion battery leaching liquid through one-step reduction method, used for hydrogen production, and magnetic separation of lithium elements, solving the problems of complex process and high purity requirements in the existing technology, and achieving high efficiency and green lithium batteries Recycling and hydrogen production.
Patent Information
- Application Number
- CN202410966157.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-07-18
AI Technical Summary
In the prior art, waste lithium-ion batteries have complex recycling processes, requiring separate metal elements, resulting in long process and high purity requirements, making it difficult to achieve efficient recycling.
A NiFeCoMnAl alloy catalyst was prepared from the lithium-ion battery leaching solution by one-step reduction method, which was used to produce hydrogen and magnetically separate lithium elements, avoiding complex separation and purification processes.
The recycling process is simplified, costs are reduced, and efficient and stable hydrogen production and priority recycling of lithium elements are achieved, which is in line with the concept of green production.
Smart Images

Figure CN119016061A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of recycling waste lithium-ion batteries, and in particular to a method for preparing a catalyst using waste lithium-ion batteries and an application of the catalyst in hydrogen production. Background Art
[0002] At present, the recycling of waste lithium-ion batteries mainly adopts pyrometallurgical or hydrometallurgical methods to separate the metal elements separately, that is, to obtain single metal elements such as lithium, cobalt, nickel, manganese, copper, aluminum, and iron, or to separate the groups to obtain a mixture of nickel, cobalt, and manganese to prepare new precursor materials.
[0003] For example, Gao et al. used formic acid as the leaching agent and H2O2 as the reducing agent to leach LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, first add NaOH to adjust the pH to 6.45 and then add ammonia to precipitate Al 3+ ; Then, the pH was adjusted and vacuum filtered to obtain a mixture of Ni(OH)2, Co(OH)2 and Mn(OH)2; finally, formic acid was used to adjust the mixture to neutrality, and Na2CO3 was added to obtain Li2CO3 precipitation. After removing Cu from the lithium-ion battery leachate, Li et al. extracted 100% of Fe and 40.3% of Mn to synthesize Fe-doped lithium ion sieve, and co-precipitated Ni, Co and the remaining Mn to prepare Ni x Co y Mn 1-x-y (OH)2 as a precursor for ternary positive electrode materials.
[0004] The individual separation of metal elements requires leaching or roasting the cathode powder first, and then separating the various elements by precipitation, extraction, etc. In order to obtain high metal purity, the process is long. The preparation of battery precursors requires the removal of substances such as iron, copper and carbon in the solution. According to the quality requirements of ternary battery precursors, the content of iron and copper must be less than 0.03% of the total amount of nickel, cobalt and manganese, so it is difficult to remove them.
[0005] Therefore, whether it is separating a single metal element or preparing a precursor, there are extremely high requirements for product purity, which makes the recycling process very complicated. Summary of the invention
[0006] In order to overcome the problems existing in the above prior art, the purpose of the present invention is to provide a method for preparing a catalyst using waste lithium-ion batteries and its application in hydrogen production. The method avoids the separation and purification process of metal elements in the process of recovering waste lithium ions, and adopts a one-step reduction method to prepare a NiFeCoMnAl alloy catalyst from a lithium-ion battery leachate. The catalyst can efficiently and stably decompose chemical hydrogen storage materials to produce hydrogen, and separates the most expensive lithium element in the waste lithium-ion batteries.
[0007] In order to achieve the above object, the technical solution adopted by the present invention is:
[0008] A method for preparing a hydrogen production catalyst using waste lithium-ion batteries comprises the following steps:
[0009] Step 1: using a sulfuric acid and hydrogen peroxide leaching system at 60° C. to 80° C. to leach the waste lithium-ion battery positive electrode powder to obtain a leaching solution containing metal ions of lithium, nickel, cobalt and manganese;
[0010] Step 2: dissolving the leaching solution, iron salt and surfactant in water, adjusting the pH value, and stirring sufficiently to mix the substances evenly to obtain a mixed solution;
[0011] Step 3: adding sodium borohydride to the mixed solution to obtain a black suspension, i.e., NiFeCoMnAl catalyst; (through sodium borohydride reduction, Ni, Fe, Co, Mn, and Al are reduced and converted into an alloy catalyst of NiFeCoMnAl, while the lithium element is not reduced and still exists in the solution).
[0012] Furthermore, in step 1, the process of obtaining the positive electrode powder is as follows:
[0013] Using saturated sodium chloride aqueous solution to soak 811, 523, 333 series of ternary waste lithium-ion batteries to discharge them, opening the shell and taking out the positive electrode sheet, using a muffle furnace to calcine the positive electrode sheet at 400-550° C. to obtain positive electrode powder;
[0014] Furthermore, any one of the 811, 523, and 333 series of waste ternary lithium-ion battery positive electrode powders is selected for leaching.
[0015] Furthermore, during the leaching process, the liquid-to-solid ratio of the leaching solution to the positive electrode powder is 50-10 mL / g. In step 2, the specific preparation steps of the NiFeCoMnAl catalyst prepared by the co-reduction method are as follows:
[0016] Take the leachate, ferrous sulfate heptahydrate, and polyvinyl pyrrolidone (PVP) and dissolve them in 3-8 mL of solution, adjust the pH to 6-9, stir well at 5-25° C., and then immediately add excess sodium borohydride to the solution;
[0017] The amount of iron added is 1:5 to 5:1 (molar ratio) of the nickel content;
[0018] During the catalyst preparation process, the concentration of PVP is 10-60 g / L, and the solution is stirred for 10-30 minutes after addition.
[0019] In step 3, sodium borohydride is added to the solution to reduce nickel, iron and cobalt metal ions to prepare a NiFeCoMnAl alloy catalyst; the amount of sodium borohydride is 7 times the total amount of nickel, iron, cobalt, aluminum and manganese metal substances.
[0020] NiFeCoMnAl catalyst is used for hydrogen production; the NiFeCoMnAl catalyst (black solid powder) is separated by centrifugation, the remaining lithium-containing solution is evaporated and concentrated, and then sodium carbonate or sodium phosphate is added to precipitate lithium, and chemical hydrogen storage materials are added to the catalyst to produce hydrogen.
[0021] Catalyze the decomposition of chemical hydrogen storage materials to produce hydrogen in the presence of 0-3 mol / L sodium hydroxide and 50-80°C;
[0022] As the element with the highest unit price in the battery, lithium still exists in the solution without being reduced. The catalyst is separated from the solution by using its magnetism, and the solution contains lithium. After the lithium-containing solution is evaporated and concentrated, sodium carbonate or sodium phosphate is added to precipitate lithium. The lithium element is extracted from the solution to realize the value-added utilization of waste lithium-ion batteries.
[0023] According to the molar ratio of lithium to sodium phosphate or sodium carbonate in the lithium-containing solution being 3:(2-5.5), sodium phosphate or sodium carbonate is added to the lithium-containing solution, the precipitate is aged at 70-100° C. for 0.5-2 h, and the lithium phosphate or lithium carbonate is obtained by filtering and washing;
[0024] The obtained catalyst was washed with water and ethanol three times respectively, and dried under hydrogen and argon atmospheres.
[0025] Furthermore, the chemical hydrogen storage material is any one of sodium borohydride, ammonia borane and hydrazine hydrate.
[0026] Furthermore, the specific steps of decomposing the chemical hydrogen storage material are as follows:
[0027] Further, the concentration of sodium hydroxide in the solution is controlled to be 0 to 3 mol / L to decompose the chemical hydrogen storage material;
[0028] Further, the solution temperature is controlled at 50 to 80°C;
[0029] Furthermore, the molar ratio of the chemical hydrogen storage material to the catalyst is controlled to be 10:1 to 100:1, and the chemical hydrogen storage material is added to perform a decomposition reaction.
[0030] Beneficial effects of the present invention:
[0031] The present invention discloses a method for preparing a hydrogen production catalyst using waste lithium ion batteries. Compared with the existing process of using waste ion batteries to produce single metals such as lithium, cobalt, nickel, and manganese or to prepare new ternary precursors, the process of preparing catalysts from waste lithium ion batteries is simple, without going through complicated separation and purification steps, and directly adopts a one-step reduction method to obtain the catalyst, thereby reducing the cost of recycling and the amount of chemical reagents used. The catalyst is used to produce hydrogen, so both the process itself and the product (i.e., hydrogen) are in line with the concept of green production.
[0032] In addition, the metal elements such as nickel, cobalt and manganese in the waste lithium-ion batteries are used to prepare hydrogen production catalysts. The catalysts have good hydrogen production performance and reuse performance, realizing the high added value utilization of waste lithium-ion batteries. At the same time, lithium, the most expensive element in waste lithium-ion batteries, can be separated and reused after the catalyst is prepared. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 It is a flow chart of the present invention.
[0034] Figure 2 The invention is a process flow chart.
[0035] Figure 3 The positive electrode powder obtained by lithium battery calcination. (a) is the positive electrode sheet before calcination, (b) is the positive electrode sheet after calcination, (c) is the aluminum foil after peeling, and (d) is the positive electrode powder.
[0036] Figure 4 The leachate obtained by leaching.
[0037] Figure 5 This is the actual leaching rate result of lithium battery during the leaching process.
[0038] Figure 6 This is a physical picture of the catalyst preparation.
[0039] Figure 7 The SEM image of the catalyst and the EDS element distribution map of each element.
[0040] Figure 8 This is the catalyst reduction rate diagram.
[0041] Fig. 9 This is a diagram of the catalytic effect of the catalyst. DETAILED DESCRIPTION
[0042] The present invention will be further described in detail below in conjunction with the accompanying drawings.
[0043] See also Figure 1The present invention discloses a method for preparing a hydrogen production catalyst using waste lithium-ion batteries, comprising the following steps:
[0044] S1. Leach the cathode powder of the ternary waste lithium-ion battery in a system of sulfuric acid and hydrogen peroxide, stir for 2 hours at 50-80°C and a liquid-solid ratio of 20-100 g / L to obtain a ternary waste lithium-ion battery leachate. Figure 4 .
[0045] The NCM models of ternary waste lithium-ion batteries are 811, 523 and 333;
[0046] The process of obtaining positive electrode powder is as follows:
[0047] Use saturated sodium chloride aqueous solution to soak 811, 523, 333 series of ternary waste lithium-ion batteries to discharge the batteries, remove the outer shell and take out the positive electrode sheet, and use a muffle furnace to calcine the positive electrode sheet at 400-550℃ to obtain positive electrode powder. Figure 3 (a) is the positive electrode sheet before calcination, (b) is the positive electrode sheet after calcination, (c) is the aluminum foil after peeling, and (d) is the positive electrode powder.
[0048] S2. Take a certain amount of ternary waste ion battery leachate, ferrous sulfate heptahydrate and PVP, adjust the pH value, stir for 10-30 minutes, and quickly add excess sodium borohydride to obtain a black catalyst. Figure 6 .
[0049] S3. Take a certain amount of catalyst and add it to 0-3 mol / L sodium hydroxide solution, control the temperature to 50-80° C., control the molar ratio of chemical hydrogen storage material and catalyst to 10:1-100:1, and add chemical hydrogen storage material to produce hydrogen.
[0050] The chemical hydrogen storage material is any one of formic acid, sodium borohydride, ammonia borane and hydrazine hydrate.
[0051] See also Figure 1 In another feasible implementation case of the present invention, the following is adaptively modified according to the situation. Use sulfuric acid and hydrogen peroxide to leach different types of ternary waste lithium-ion battery positive electrode powder, stir at 50-80°C and 20-100g / L for 2 hours to obtain a ternary waste lithium-ion battery leachate. Take a certain amount of ternary waste ion battery leachate, ferrous sulfate heptahydrate and PVP, adjust the pH value and stir for 10-30 minutes, quickly add an excess of sodium borohydride to obtain a black catalyst. Figure 6. A magnet is used to separate the catalyst and the lithium solution to achieve the priority recovery of lithium. The obtained catalyst is rinsed with water and ethanol three times each, and dried under hydrogen and argon atmospheres. No additional reagents or solutions are required in the experiment, avoiding excessive waste of reagents. Take a certain amount of catalyst and add it to 0-3 mol / L sodium hydroxide solution, control the temperature to 50-80°C, control the molar ratio of chemical hydrogen storage material and catalyst to 10:1-100:1, and add chemical hydrogen storage material for decomposition reaction to produce hydrogen. The nickel, cobalt, manganese and other metal ions in waste lithium-ion batteries are not separated and purified, but directly converted into NiFeCoMnAl catalysts by a one-step reduction method, which are used to catalyze the production of hydrogen by chemical hydrogen storage materials. Compared with conventional recycling methods, the cost of recycling is reduced. More importantly, the process for preparing the catalyst is simple, the amount of reagents consumed is small, and the catalyst can be used to produce hydrogen. Therefore, both the process itself and the product (i.e., hydrogen) are in line with the concept of green development. See Figure 2 is a process flow chart of the present invention, Fig. 9 The catalyst prepared by the present invention changes the hydrogen production rate and hydrogen selectivity over time when catalyzing hydrazine hydrate to produce hydrogen at different sodium hydroxide concentrations and temperatures. The present invention avoids the cumbersome steps and redundant reagents of the traditional recovery process. The catalyst prepared by the one-step co-reduction method can preferentially recover lithium and realize stable and efficient decomposition to produce hydrogen, providing a new way for the value-added utilization of lithium batteries.
[0052] Embodiment 1:
[0053] The 523-type ternary waste lithium-ion battery was discharged, the positive electrode sheet was taken out after the shell was removed, and the positive electrode sheet was calcined at 500° C. in a muffle furnace to obtain positive electrode powder;
[0054] Use 4 mol / L sulfuric acid and 6% hydrogen peroxide to leach the waste lithium-ion battery positive electrode powder at 80°C and 50 g / L, stir for 2 hours, and obtain the ternary waste lithium-ion battery leachate. Figure 5 The elements Li, Ni and Co in the leaching solution were analyzed by ICP-OES, and the leaching rates of various elements were calculated to be higher than 95%.
[0055] Take 2mL of ternary waste ion battery leachate, 0.3g PVP, add ferrous sulfate according to the nickel-iron ratio of 1:1, adjust pH to 8 with sodium hydroxide solution, then dilute the above solution to 15mL and stir for 30min. Quickly add excess sodium borohydride to obtain a black catalyst. Use a magnet to separate the catalyst and lithium solution to achieve preferential recovery of lithium. Add 1mol / L sodium hydroxide solution to the catalyst, control the temperature to 60℃, control the molar ratio of ammonia borane and catalyst to 20:1, and add ammonia borane for decomposition reaction. The hydrogen selectivity is 83%.
[0056] Embodiment 2:
[0057] The 811 type ternary waste lithium-ion battery was discharged, the positive electrode sheet was taken out after the shell was removed, and the positive electrode sheet was calcined at 500°C in a muffle furnace to obtain positive electrode powder;
[0058] 3 mol / L sulfuric acid and 6% hydrogen peroxide were used to leach the cathode powder of waste lithium-ion batteries at 80°C and 40 g / L, and stirred for 2 hours to obtain a ternary waste lithium-ion battery leachate. The elements Li, Ni and Co in the leachate were analyzed by ICP-OES, and the leaching rates of various elements were calculated to be higher than 90%.
[0059] Take 2mL of ternary waste ion battery leachate, 0.3g PVP, add ferrous sulfate in a nickel-iron ratio of 1:1, adjust pH to 9 with sodium hydroxide solution, and then dilute the solution to 15mL. Quickly add excess sodium borohydride to obtain a black catalyst with a reduction rate of more than 97% for nickel, cobalt, manganese and aluminum (see Figure 8 ). A magnet is used to separate the catalyst and lithium solution to achieve preferential recovery of lithium.
[0060] 0.2g of catalyst was added to 0.5mol / L sodium hydroxide solution, the temperature was controlled to 60°C, the molar ratio of hydrazine hydrate to catalyst was controlled to 10:1, and hydrazine hydrate was added for decomposition reaction. The hydrogen selectivity was 85%.
[0061] See also Figure 8 This is a catalytic effect diagram of the present invention. The present invention realizes the green and high value-added utilization of waste lithium ions through a simple metallurgical process. The present invention adopts a process of leaching first and then co-reduction to convert the Ni in the high-nickel waste lithium ion battery leachate into 2+ 、Co 2+ , Mn 2+ The metal ions are reduced to catalysts for catalytic hydrogen production by chemical hydrogen storage materials, while the unreduced Li + After separation, it is used to prepare new lithium-ion batteries. This method significantly shortens the recycling process of waste lithium ions and realizes the high added value utilization of various metal ions. In addition, the catalyst prepared by this method has better performance in catalyzing chemical materials to produce hydrogen than other non-precious metal nickel-based catalysts.
[0062] Figure 7 The SEM and EDS element distribution diagrams of the catalyst show that the Ni x Fe y The morphology of CoMnAl catalyst is as follows Figure 7As shown in the figure, it can be seen that the particle size of the catalyst is small, at the nanometer level, and the distribution of each element in the catalyst is uniform, indicating that the prepared catalyst is an alloy of Ni, Fe, Co, Mn, and Al.
[0063] The changes of the hydrogen production rate and hydrogen selectivity over time when the synthesized catalyst catalyzes the production of hydrogen from hydrazine at different sodium hydroxide concentrations and temperatures. In general, increasing the sodium hydroxide concentration can increase the selectivity of hydrogen (i.e., the number of moles of hydrogen in the catalytic product accounts for the number of moles of hydrogen in hydrazine), but has little effect on the hydrogen production rate, while increasing the temperature can effectively increase the hydrogen production rate and hydrogen selectivity.
[0064] The above contents are only for explaining the technical idea of the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.
Claims
1. A method for preparing a hydrogen production catalyst using waste lithium-ion batteries, characterized in that: The steps include: Step 1: using a sulfuric acid and hydrogen peroxide leaching system at 60° C. to 80° C. to leach the waste lithium-ion battery positive electrode powder to obtain a leaching solution containing metal ions of lithium, nickel, cobalt and manganese; Step 2: dissolving the leaching solution, iron salt and surfactant in water, adjusting the pH value, and stirring thoroughly to mix the substances evenly to obtain a mixed solution; Step 3: Add sodium borohydride to the mixed solution to obtain a black suspension, namely, the NiFeCoMnAl catalyst.
2. The method for preparing a hydrogen production catalyst using waste lithium-ion batteries according to claim 1, characterized in that: In step 1, the process of obtaining the positive electrode powder is as follows: Using saturated sodium chloride aqueous solution to soak 811, 523, 333 series of ternary waste lithium-ion batteries to discharge them, opening the shell and taking out the positive electrode sheet, using a muffle furnace to calcine the positive electrode sheet at 400-550° C. to obtain positive electrode powder; Any one of the 811, 523, 333 series of waste ternary lithium-ion battery positive electrode powders is selected for leaching.
3. The method for preparing a hydrogen production catalyst using waste lithium-ion batteries according to claim 2, characterized in that: During the leaching process, the liquid-to-solid ratio of the leaching solution to the positive electrode powder is 50-10 mL / g.
4. The method for preparing a hydrogen production catalyst using waste lithium-ion batteries according to claim 1, characterized in that: In step 2, the specific preparation steps of the NiFeCoMnAl catalyst prepared by the co-reduction method are as follows: Take the leachate, ferrous sulfate heptahydrate, and polyvinyl pyrrolidone (PVP) and dissolve them in 3-8 mL of solution, adjust the pH to 6-9, stir well at 5-25° C., and then immediately add excess sodium borohydride to the solution; The amount of iron added is 1:5 to 5:1 of the nickel content; During the catalyst preparation process, the concentration of PVP is 10-60 g / L, and the solution is stirred for 10-30 minutes after addition.
5. The method for preparing a hydrogen production catalyst using waste lithium-ion batteries according to claim 4, characterized in that: In step 3, sodium borohydride is added to the solution to reduce nickel, iron and cobalt metal ions to prepare a NiFeCoMnAl alloy catalyst; the amount of sodium borohydride is 7 times the total amount of nickel, iron, cobalt, aluminum and manganese metal substances.
6. The NiFeCoMnAl catalyst prepared according to the method according to any one of claims 1 to 5 is used for hydrogen production, characterized in that: The catalyst and the lithium-containing solution are separated by centrifugation, sodium carbonate or sodium phosphate is added to the lithium-containing solution after evaporation and concentration, and chemical hydrogen storage materials are added to the catalyst to produce hydrogen; According to the molar ratio of lithium to sodium phosphate or sodium carbonate in the lithium-containing solution being 3:(2-5.5), sodium phosphate or sodium carbonate is added to the lithium-containing solution, the precipitate is aged at 70-100° C. for 0.5-2 h, and the lithium phosphate or lithium carbonate is obtained by filtering and washing; The obtained catalyst was washed with water and ethanol three times respectively, and dried under hydrogen and argon atmospheres.
7. The NiFeCoMnAl catalyst according to claim 6 is used for hydrogen production, characterized in that: Under the conditions of 0-3 mol / L sodium hydroxide and 50-80°C, the chemical hydrogen storage material is catalyzed to decompose and produce hydrogen.
8. The NiFeCoMnAl catalyst according to claim 7 is used for hydrogen production, characterized in that: The chemical hydrogen storage material is any one of sodium borohydride, ammonia borane and hydrazine hydrate.
9. The NiFeCoMnAl catalyst according to claim 7 is used for hydrogen production, characterized in that: The molar ratio of the chemical hydrogen storage material to the catalyst is controlled to be 10:1 to 100:1, and the chemical hydrogen storage material is added to carry out a decomposition reaction.
Citation Information
Patent Citations
Method for recycling valuable metal in waste nickel-cobalt-manganese ternary lithium-ion battery
CN108470951A
Waste Ni-Co-Mn lithium manganate positive electrode material recycling method
CN108539309A
Supported catalyst for hydrogen production through hydrolysis of sodium borohydride solution as well as preparation method and application of supported catalyst
CN113171776A
Method of recovering hydrogen storage alloy constituent element
JP2005113226A
Method for recovering waste lithium battery positive electrode material
WO2022062675A1
Cited By
Method for preparing lithium iron phosphate by recycling waste lithium iron phosphate batteries and application