Locomotive single rocker arm rear axle machining process

By combining low-temperature Dacromet coating with replaceable rotating tips, the problem of reduced hardness caused by medium-temperature Dacromet coating was solved, thus improving the mechanical performance of the locomotive's single-rocker rear axle.

CN119017010APending Publication Date: 2024-11-26CHONGQING MEIXIN YINGSHEN MACHINERY CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411049748.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

In the existing technology, the medium-temperature Dacromet plating process of the rear wheel axle of the single rocker arm of the locomotive leads to a decrease in hardness in the high-frequency quenching area, resulting in a decline in mechanical properties and early failure.

Method used

The low-temperature Dacromet process is adopted, and the drying and sintering temperatures are controlled within the range of 230-260℃. Replaceable rotating tips are used to fix the product during the fine grinding stage to prevent the coating from peeling off.

Benefits of technology

This improved the product's hardness, meeting technical requirements, preventing hardness reduction, and extending the product's service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119017010A_ABST
    Figure CN119017010A_ABST
Patent Text Reader

Abstract

The invention relates to the field of machining, in particular to a machining technology for a single-rocker-arm rear axle of a locomotive. Comprising the following steps that S1, a blank is subjected to receiving inspection; s2, rough machining; s3, hardening and tempering; s4, finish machining; s5, quenching and flaw detection; s6, Dacromet plating at a low temperature; s7, the rod part is finely ground; s8, cleaning and rust-proof treatment are conducted, wherein low-temperature Dacromet plating is conducted by controlling the temperature within the range of 230-260 DEG C in the drying and sintering process; by the adoption of the machining process for the single-rocker-arm rear axle of the locomotive, products can have good strength and anti-rust performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of mechanical processing, and in particular to a processing technology for a rear wheel shaft of a locomotive single rocker arm. Background Art

[0002] The rear wheel axle is a key component of a motorcycle. Its structure includes a flying disc in the middle and a long shaft and a short shaft at both ends of the flying disc. When in use, it is partially exposed to the air and requires good strength and rust resistance. In the prior art, the surface treatment of Dacromet plating generally adopts a medium temperature (300-350℃) Dacromet plating process. The medium temperature Dacromet process adopts 300-350 degrees Celsius plating baking to solidify the Dacromet coating, which will produce secondary tempering phenomenon in the high-frequency quenching area. The high tempering temperature will reduce the hardness of the high-frequency quenching area by 7-9HRC, reduce the surface hardness of the part, reduce the mechanical properties, and cause early failure. Summary of the invention

[0003] The invention aims to provide a locomotive single rocker arm rear wheel axle processing technology which can improve product performance.

[0004] The invention provides a locomotive single rocker arm rear wheel axle processing technology, comprising the following steps: S1, blank receiving inspection; S2, rough machining; S3, quenching and tempering; S4, fine machining; S5, quenching and flaw detection; S6, low-temperature Dacromet plating; S7, fine grinding of the rod; S8, cleaning and rust prevention treatment.

[0005] Furthermore, the Dacromet plating in step S6 is low-temperature Dacromet, and the temperature of the product is controlled within the range of 230-260° C. during the drying and sintering process.

[0006] Furthermore, in the step S7, after the product is fixed by using a replaceable rotating center, the short shaft and long shaft are finely ground.

[0007] Further, the rough machining of step S2 includes the following steps: S2.1, using a CNC lathe to rough turn the outer circle and end face of the short shaft, the CNC lathe speed is 800-900r / min, the feed amount is F0.2-F0.5, the chuck pressure is 1-2Mpa, and the coolant level is normal; S2.2, using a CNC lathe to rough turn the outer circle and end face of the long shaft, the CNC lathe speed is 800-900r / min, the feed amount is F0.2-F0.5, the chuck pressure is 1-2Mpa, and the coolant level is normal; S2.3, using a drilling machine to roughly drill the center hole, the drilling machine speed is 1100-1300r / min, the feed amount is F60-F70, the chuck hydraulic box pressure is 3-5Mpa, and the drilling and milling fluid concentration is 2-5%.

[0008] Furthermore, after the quenching and tempering in step S3, the product undergoes a heat treatment process of quenching and high-temperature tempering, and the hardness HRC of the product is 26-36, the tempered troostite is level 1-4, the tensile strength is 850-1050MPa, the elongation is not less than 12%, and the yield strength is not less than 675MPa.

[0009] Further, the finishing of step S4 includes the following steps: S4.1, finishing the outer circle, end face, inner hole and external thread of the long shaft rod; S4.2, finishing the outer circle, end face, inner hole and external thread of the short shaft rod; S4.3, drilling, reaming and chamfering the mounting hole of the flying disc; S4.4, drilling the stop hole; S4.5, deburring; S4.6, knurling the key teeth.

[0010] Furthermore, in step S5, a high-frequency quenching furnace is used for quenching, the power of the high-frequency quenching furnace is 70-110 kW, the heating time is 3-6 s, and the concentration of the quenching liquid is 3-6%.

[0011] Furthermore, the Dacromet plating in step S6 is low-temperature Dacromet, and the temperature of the product is controlled within the range of 240-250° C. during the drying and sintering process.

[0012] Furthermore, after the product has gone through step 6, the hardness reaches 54-58HRC, and there is no obvious change in appearance after a 240-hour salt spray test.

[0013] Furthermore, the anti-rust treatment in step S8 is to wrap and cover the fine grinding part with anti-rust paper.

[0014] The advantages of the present invention are: the product adopts a low-temperature Dacromet process during the drying and sintering process, the temperature is controlled within the range of 230-260°C, and secondary tempering is formed. Due to the relatively low temperature, the hardness is reduced by 2-3HRC, which can meet the product technical requirements, and the product adopts a replaceable rotating top in the fine grinding process stage. The top rotates with the product without relative movement, which can avoid the shedding of the coating from the center hole to the corner. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 The figure is a flow chart of the processing technology of the rear wheel axle of the single rocker arm of a locomotive according to the present invention. DETAILED DESCRIPTION

[0016] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments:

[0017] according to Figure 1 As shown, the locomotive single rocker arm rear wheel axle processing technology in this scheme includes the following steps:

[0018] S1, the blanks are inspected upon receipt, including the inspection of the geometric dimensions and chemical composition of the blanks. The sampling method is adopted, and 1-3 pieces are randomly inspected in a batch.

[0019] S2, rough machining, specifically includes the following steps: S2.1, use CNC lathe to rough turn the outer circle and end face of the short shaft, the CNC lathe speed is 800-900r / min, the feed amount is F0.2-F0.5, the chuck pressure is 1-2Mpa, and the coolant level is normal; S2.2, use CNC lathe to rough turn the outer circle and end face of the long shaft, the CNC lathe speed is 800-900r / min, the feed amount is F0.2-F0.5, the chuck pressure is 1-2Mpa, and the coolant level is normal; S2.3, use a drilling machine to roughly drill the center hole, the drilling machine speed is 1100-1300r / min, the feed amount is F60-F70, the chuck hydraulic box pressure is 3-5Mpa, and the drilling and milling fluid concentration is 2-5%.

[0020] S3, quenching and tempering, the specific indicators are that after the product has undergone quenching and high-temperature tempering heat treatment processes, the product's hardness HRC is 26-36, the tempered troostite is level 1-4, the tensile strength is 850-1050MPa, the elongation is not less than 12%, and the yield strength is not less than 675MPa.

[0021] S4, finishing, which specifically includes the following steps: S4.1, finishing the outer circle, end face, inner hole and external thread of the long shaft rod; S4.2, finishing the outer circle, end face, inner hole and external thread of the short shaft rod; S4.3, drilling, reaming and chamfering the mounting hole of the flying disc; S4.4, drilling the stop hole; S4.5, deburring; S4.6, knurling the key teeth.

[0022] S5, quenching and flaw detection, where quenching is done using a high-frequency quenching furnace with a power of 70-110kw, a heating time of 3-6s, and a quenching liquid concentration of 3-6%. Then the product is inspected.

[0023] S6, low temperature Dacromet plating; specifically low temperature Dacromet, the product temperature is controlled within the range of 230-260℃ during drying and sintering. Furthermore, the product temperature is controlled within the range of 240-250℃ during drying and sintering. The hardness reaches 54-58HRC, and there is no obvious change in appearance after 240h salt spray test.

[0024] S7, fine grinding of the rod, after fixing the product with a replaceable rotating center, fine grinding of the short and long shaft rods. Marking on the product after fine grinding, and general inspection of the product after marking.

[0025] S8, cleaning oil stains and anti-rust treatment, where the anti-rust treatment is to wrap and cover the fine grinding parts with anti-rust paper, and finally pack the products into boxes and put them into storage.

[0026] The advantages of the present invention are: the product adopts a low-temperature Dacromet process during the drying and sintering process, the temperature is controlled within the range of 230-260°C, and secondary tempering is formed. Due to the relatively low temperature, the hardness is reduced by 2-3HRC, which can meet the product technical requirements, and the product adopts a replaceable rotating top in the fine grinding process stage. The top rotates with the product without relative movement, which can avoid the shedding of the coating from the center hole to the corner.

[0027] The above is only an embodiment of the present invention, and the common knowledge such as the known specific structure and characteristics in the scheme is not described in detail here. It should be pointed out that for those skilled in the art, several modifications and improvements can be made without departing from the structure of the present invention, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent.

Claims

1. The processing technology of the rear wheel shaft of a single rocker arm of a locomotive is characterized by , including the following steps: S1, blank receiving inspection; S2, roughing; S3, conditioning; S4, finishing; S5, quenching and flaw detection; S6, low-temperature Dacromet coating; S7, fine grinding of the shaft; S8, cleaning and rust-proof treatment.

2. The locomotive single rocker arm rear wheel axle processing technology according to claim 1 is characterized in that: The Dacromet plating in step S6 is low-temperature Dacromet, and the temperature of the product is controlled within the range of 230-260° C. during the drying and sintering process.

3. The locomotive single rocker arm rear wheel axle processing technology according to claim 1 is characterized in that: In step S7, after the product is fixed by using a replaceable rotating center, the short shaft and long shaft are finely ground.

4. The locomotive single rocker arm rear wheel axle processing technology according to claim 1 is characterized in that: The rough machining of step S2 comprises the following steps: S2.1, use CNC lathe to rough turn the outer circle and end face of the short shaft, the CNC lathe speed is 800-900r / min, the feed rate is F0.2-F0.5, the chuck pressure is 1-2Mpa, and the coolant level is normal; S2.2, use CNC lathe to rough turn the outer circle and end face of the long shaft, the CNC lathe speed is 800-900r / min, the feed rate is F0.2-F0.5, the chuck pressure is 1-2Mpa, and the coolant level is normal; S2.3, use a drilling machine to roughly drill the center hole, the drilling machine speed is 1100-1300r / min, the feed rate is F60-F70, the hydraulic box pressure is 3-5Mpa, and the drilling and milling fluid concentration is 2-5%.

5. The locomotive single rocker arm rear wheel axle processing technology according to claim 1 is characterized in that: After the quenching and tempering in step S3, the product undergoes a heat treatment process of quenching and high-temperature tempering, and the hardness HRC of the product is 26-36, the tempered troostite is 1-4 level, the tensile strength is 850-1050MPa, the elongation is not less than 12%, and the yield strength is not less than 675MPa.

6. The motorcycle single rocker arm rear wheel axle processing technology according to claim 1, characterized in that: The finishing process of step S4 comprises the following steps: S4.1, finish turning the outer circle, end face, inner hole and external thread of the long shaft; S4.2, finish turning the outer circle, end face, inner hole and external thread of the short shaft; S4.3, drilling, reaming, and chamfering the mounting holes for the discs; S4.4, drilling the anti-rotation hole; S4.5, deburring; S4.6, knurled key teeth.

7. The locomotive single rocker arm rear wheel axle processing technology according to claim 1 is characterized in that: In step S5, a high-frequency quenching furnace is used for quenching, the power of the high-frequency quenching furnace is 70-110 kW, the heating time is 3-6 seconds, and the concentration of the quenching liquid is 3-6%.

8. The locomotive single rocker arm rear wheel axle processing technology according to claim 2 is characterized by: The Dacromet plating in step S6 is low-temperature Dacromet, and the temperature of the product is controlled within the range of 240-250° C. during the drying and sintering process.

9. The locomotive single rocker arm rear wheel axle processing process according to claim 8, characterized in that: After the product has gone through step 6, the hardness reaches 54-58HRC, and there is no obvious change in appearance after a 240-hour salt spray test.

10. The motorcycle single rocker arm rear wheel axle processing technology according to claim 2, characterized in that: The rust-proof treatment in step S8 is to wrap and cover the fine grinding part with rust-proof paper.

Citation Information

Patent Citations

  • Manufacture method of vehicular air conditioning condenser

    CN103084316A

  • Machining technology for automobile transmission shaft

    CN110116300A

  • Double-end stud for connecting roots of blades of wind turbine generator and machining method of double-end stud

    CN116877555A

  • Movable center for machine tool

    CN215919927U

  • Production of gear by induction hardening

    JP1997272920A