Preparation method of porous polyethylene implant

The preparation of large-grained porous polyethylene implants through underwater granulation process solves the problems of infection and tissue growth limitation caused by small pore size in the prior art, and improves the stability and biological of the implant through functional modification. performance.

CN119017728AActive Publication Date: 2024-11-26SHANGHAI POLLY MEDICAL MATERIALS CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202411514789.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-29
Publication Date
2024-11-26
Estimated Expiration
2044-10-29

AI Technical Summary

Technical Problem

The average pore size of the existing pores of porous polyethylene implants is small, which can easily cause infection and limit tissue growth. The diameter of the polyethylene powder used in the sintering method is usually below 100 μm, resulting in low long-term stability of the implant and low cell adhesion efficiency.

Method used

Polyethylene particles with an average particle size of 300~800μm were prepared by underwater granulation process, and sintered and molded in the mold to form porous polyethylene implants with larger pore sizes. At the same time, functional modification can be carried out to enhance antibacterial and Antioxidant capacity.

Benefits of technology

The average pore size of porous polyethylene implants is improved, the growth and vascularization of tissue cells is promoted, the risk of infection is reduced, and the service life and biocompatibility of the implant is improved through functional modification.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119017728A_ABST
    Figure CN119017728A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of high polymer materials, and particularly relates to a preparation method of a porous polyethylene implant, which comprises the following steps: a) carrying out melt extrusion on polyethylene, and then carrying out underwater granulation to obtain polyethylene particles with the average particle size of 300-800 [mu] m; and b) filling the polyethylene particles into a mold, sintering, molding and cooling to obtain the porous polyethylene implant. The preparation method comprises the following steps: firstly, preparing large polyethylene particles with a certain particle size by adopting an underwater granulation process, then sintering the large polyethylene particles in a mold, and mutually contacting and bonding the large polyethylene particles in the sintering process to form rich and large-size three-dimensional holes. By adopting the method disclosed by the invention, the porous polyethylene implant with a relatively large aperture can be prepared, and the relatively large aperture can promote tissue cells to grow in, so that the implant is not easy to displace, the vascularization of an implanted part can be promoted, and the infection risk is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polymer materials, and in particular relates to a method for preparing a porous polyethylene implant. Background Art

[0002] Polyethylene is a polymer compound, which is polymerized from ethylene monomers. It can be generally divided into low-density polyethylene, high-density polyethylene and ultra-high molecular weight polyethylene. Polyethylene has the advantages of good toughness, wear resistance, strong chemical resistance and good biological safety, so it is widely used in the medical field. For example, medical polyethylene is used in infusion tubes, blood transfusion bags, artificial implants and other devices.

[0003] With polyethylene material as the matrix, a three-dimensional microporous structure can be formed inside it by regulating the molding process, so that it can have both the excellent comprehensive performance of polyethylene material and the advantages of porous materials, greatly expanding the application field of polyethylene and achieving the goal of multifunctionality.

[0004] Compression molding-template leaching method and sintering method are two common methods for preparing porous polyethylene. Compression molding-template leaching method usually involves physically blending polyethylene powder and porogen raw materials in a certain proportion, then adding them to a mold, and compression molding them on a hot pressing molding device, and finally removing the porogen to obtain porous polyethylene. However, this method usually has the disadvantages that the pore parameters are difficult to adjust and the residual porogen will harm the human body; the sintering method refers to using polyethylene powder as raw material, subjecting it to a certain temperature and pressure in the mold, the powders contact and bond with each other to form a sintering neck, and retaining the voids by rapid cooling before the particles are completely bonded, and finally forming a porous polyethylene with a three-dimensional porous structure; however, the diameter of the polyethylene powder used in the sintering method is usually below 100μm, and the average pore size of the sintered porous polyethylene is small (about 20~50μm), which is easy to cause infection due to bacterial residues after implantation into the human body. Foreign scholars have reported that when the average pore size of the implant is 100-250 μm, it is easier to promote tissue ingrowth and vascularization, and reduce the risk of infection. When the pore size is smaller, it will limit the degree of tissue ingrowth and easily leave bacteria. When the pore size is larger, the long-term stability of the implant will be affected, and the low cell adhesion efficiency is not conducive to cell proliferation. Domestic scholars have reported that when the pore size is greater than 100 μm, it is conducive to cell ingrowth, the transfer of nutrients and the discharge of metabolites. Domestic scholars have also reported the effect of porosity on cell adhesion and tissue growth. Too high a porosity is not conducive to cell adhesion, and the long-term stability of the scaffold will be affected; too small a porosity will hinder the ingrowth of tissue cells. Summary of the invention

[0005] In view of this, the purpose of the present invention is to provide a method for preparing a porous polyethylene implant. The method provided by the present invention improves the process of preparing porous polyethylene by traditional sintering method, and greatly increases the average pore size of the sintered product.

[0006] The present invention provides a method for preparing a porous polyethylene implant, comprising the following steps:

[0007] a) melt-extrude the polyethylene and then perform underwater granulation to obtain polyethylene particles with an average particle size of 300-800 μm;

[0008] b) filling the polyethylene particles into a mold, sintering and cooling to obtain a porous polyethylene implant.

[0009] Preferably, in step a), the polyethylene has a melt flow index of 0.5-50 g / 10 min under test conditions of 190° C. and 21.6 kg; and a weight average molecular weight of 150,000-1,500,000 g / mol.

[0010] Preferably, in step a), a plasticizer and / or a surfactant is added during the melting process.

[0011] Preferably, in step a), the plasticizer is one or more of PEG400, PEG2000 and PEG4000; the surfactant is one or more of Span 40, Tween 40 and Tween 80.

[0012] Preferably, in step a), the plasticizer accounts for 0-5% of the total mass of polyethylene, plasticizer and surfactant; the surfactant accounts for 0-5% of the total mass of polyethylene, plasticizer and surfactant.

[0013] Preferably, in step a), the melt extrusion is carried out in a twin-screw extruder, the die opening diameter of the twin-screw extruder is 300-800 μm; the melt extruded melt is cut and granulated underwater, and the cutting machine speed is 300-1200 rpm.

[0014] Preferably, in step a), the screw speed of the twin-screw extruder is 100-300 rpm, and the barrel temperature is 180-220° C.; and the water temperature of the melt during underwater cutting and granulation is 60-90° C.

[0015] Preferably, in step a), the degree of spheroidization of the polyethylene particles is 40-100%.

[0016] Preferably, in step b), the sintering temperature is 140-220° C. and the sintering time is 3-15 min.

[0017] Preferably, the preparation method further comprises: during the preparation of the porous polyethylene implant, performing functional modification on it.

[0018] Preferably, the functional modification method includes sintering modification and / or surface modification.

[0019] Compared with the prior art, the present invention provides a method for preparing a porous polyethylene implant, comprising the following steps: a) melt-extrude polyethylene and then perform underwater granulation to obtain polyethylene particles with an average particle size of 300-800 μm; b) fill the polyethylene particles into a mold, sinter and form, and cool to obtain a porous polyethylene implant. The present invention first uses an underwater granulation process to prepare large polyethylene particles with a certain particle size, and then sinter these large polyethylene particles in a mold. During the sintering process, the large polyethylene particles contact and bond with each other to form abundant and large three-dimensional holes. The method of the present invention can be used to prepare a porous polyethylene implant with a larger pore size. The larger pore size can promote the growth of tissue cells, making the implant less likely to shift, and can also promote vascularization of the implant site, reducing the risk of infection. In addition, in the preferred technical scheme provided by the present invention, the porous polyethylene implant can also be functionally modified to give it biological functions such as antibacterial and antioxidant properties, thereby further reducing the infection risk of the implant and increasing the service life of the implant. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.

[0021] Figure 1 is a scanning electron microscope image of the nearly spherical UHWMPE microparticles prepared in Example 1 of the present invention;

[0022] Figure 2 is a scanning electron microscope image of a porous polyethylene implant product prepared in Example 1 of the present invention;

[0023] Figure 3 This is a digital photo of a porous polyethylene implant product containing a functional additive coating prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0024] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] The present invention provides a method for preparing a porous polyethylene implant, comprising the following steps:

[0026] a) melt-extrude the polyethylene and then perform underwater granulation to obtain polyethylene particles with an average particle size of 300-800 μm;

[0027] b) filling the polyethylene particles into a mold, sintering and cooling to obtain a porous polyethylene implant.

[0028] In the preparation method provided by the present invention, in step a), in order to granulate the spherical microparticles mentioned in the present invention, it is necessary to keep the melt flow index of polyethylene within a certain range as much as possible. When the melt index is too low, the particles obtained by shaping are not easy to form a sphere, but are easy to form a cylinder. According to the stacking theory, the porosity of spherical particles during stacking and sintering will be higher than that of cylindrical particles; when the melt index is too high, although microparticles with good sphericity can be produced, the fluidity is too good, and the particles are easy to fuse excessively during the sintering process, resulting in a decrease in porosity. In the present invention, the melt flow index of the polyethylene is preferably 0.5~50g / 10min (190℃, 21.6kg), more preferably 2~40g / 10min, more preferably 5~35g / 10min, and most preferably 10~30g / 10min. The polyethylene after the melt flow index is optimized has improved melt flowability, higher spheroidization after granulation, and is not easy to cause excessive fusion between particles during sintering. In the present invention, the melt flow index of the polyethylene may specifically be 0.5 g / 10 min, 1 g / 10 min, 2 g / 10 min, 5 g / 10 min, 10 g / 10 min, 20 g / 10 min, 30 g / 10 min, 40 g / 10 min or 50 g / 10 min.

[0029] In the preparation method provided by the present invention, in step a), although the molecular weight of polyethylene generally does not directly affect the porosity of the product, the molecular weight is negatively correlated with the melt flow index (the larger the molecular weight, the smaller the melt index is usually), so in order to granulate the spherical microparticles mentioned in the present invention, it is also necessary to control the molecular weight of polyethylene within a certain range. In the present invention, the weight average molecular weight of the polyethylene is preferably 150,000 to 1,500,000 g / mol, more preferably 180,000 to 1,100,000 g / mol, more preferably 200,000 to 700,000 g / mol, and most preferably 250,000 to 400,000 g / mol. The polyethylene with the preferred weight average molecular weight has improved melt flowability, a higher degree of spheroidization after granulation, and is less likely to cause excessive fusion between particles during sintering. In the present invention, the weight average molecular weight of the polyethylene can be 150000 g / mol, 200000 g / mol, 250000 g / mol, 300000 g / mol, 350000 g / mol, 400000 g / mol, 450000 g / mol, 500000 g / mol, 550000 g / mol, 600000 g / mol, 650000 g / mol. l, 700000g / mol, 750000g / mol, 800000g / mol, 850000g / mol, 900000g / mol, 950000g / mol, 10 00000g / mol, 1100000g / mol, 1200000g / mol, 1300000g / mol, 1400000g / mol or 1500000g / mol.

[0030] In the preparation method provided by the present invention, in step a), a plasticizer and / or a surfactant may be selectively added during the melting process. In the present invention, the surfactant and the plasticizer are added to improve the fluidity of the polyethylene, thereby granulating microparticles with better sphericity, thereby improving the pore morphology uniformity, average pore size and porosity of the product. It should be noted that these two components are not necessarily added. If a high melt index polyethylene within the range is selected, even if these two components are not added, microparticles with good sphericity can be produced by adjusting the equipment parameters.

[0031] In the preparation method provided by the present invention, in step a), the plasticizer includes but is not limited to one or more of PEG400, PEG2000 and PEG4000, and the above-mentioned types of plasticizers have good biosafety. In the present invention, the plasticizer preferably accounts for 0-5% of the total mass of polyethylene, plasticizer and surfactant (if it exceeds 5%, the biosafety may not meet the requirements), more preferably 0.5-4.5%, more preferably 1-4%, most preferably 1.5-3.5%, after the plasticizer is added in an amount, the polyethylene has better fluidity during melt extrusion, better biosafety, and less risk after implantation in the human body. In the present invention, the plasticizer can specifically account for 0%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5% or 5% of the total mass of polyethylene, plasticizer and surfactant.

[0032] In the preparation method provided by the present invention, in step a), the surfactant includes but is not limited to one or more of Span 40, Tween 40 and Tween 80; the surfactant preferably accounts for 0-5% of the total mass of polyethylene, plasticizer and surfactant (if it exceeds 5%, the biosafety may not meet the requirements), more preferably 0.5-4.5%, more preferably 1-4%, most preferably 1.5-3.5%, after the surfactant is added in an optimal amount, the polyethylene has better fluidity during melt extrusion, better biosafety, and less risk after implantation into the human body. In the present invention, the surfactant can specifically account for 0%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5% or 5% of the total mass of polyethylene, plasticizer and surfactant.

[0033] In the preparation method provided by the present invention, in step a), the melt extrusion is carried out in a twin-screw extruder; wherein, the screw speed of the twin-screw extruder is preferably 100-300 rpm, specifically 100 rpm, 150 rpm, 200 rpm, 250 rpm or 300 rpm; the barrel temperature of the twin-screw extruder is preferably 180-220°C, specifically, the temperature of the rear section (close to the feed port) is preferably 180-200°C, specifically 180°C, 190°C or 200°C, the temperature of the middle section is preferably 190-210°C, specifically 190°C, 200°C or 210°C, and the temperature of the front section (close to the discharge port) is preferably 200-220°C, specifically 200°C, 210°C or 220°C. In the present invention, the die opening diameter of the twin-screw extruder is preferably 300-800 μm, more preferably 400-700 μm, and even more preferably 450-650 μm. After the die opening diameter is optimized, the size range of the polyethylene particles after granulation is more suitable; the die opening diameter of the twin-screw extruder can specifically be 300 μm, 350 μm, 400 μm, 450 μm, 500 μm, 550 μm, 600 μm, 650 μm, 700 μm, 750 μm or 800 μm.

[0034] In the preparation method provided by the present invention, in step a), the melt-extruded melt is cut and granulated underwater; wherein, the rotation speed of the cutter is preferably 300-1200 rpm, more preferably 400-1100 rpm, preferably 500-1000 rpm, most preferably 600-900 rpm, the preferred rotation speed of the cutter can match the preferred die opening diameter, and the polyethylene particles obtained by granulation have better spheroidization; the rotation speed of the cutter can specifically be 300 rpm, 350 rpm, 400 rpm, 450 rpm, 500 rpm, 550 rpm, 600 rpm, 650 rpm, 700 rpm, 750 rpm, 800 rpm, 850 rpm, 900 rpm, 950 rpm, 1000 rpm, 1100 rpm or 1200 rpm. In the present invention, the water temperature of the melt during underwater cutting and granulation is preferably 60-90°C, specifically 60°C, 65°C, 70°C, 75°C, 80°C, 85°C or 90°C.

[0035] In the preparation method provided by the present invention, in step a), the average particle size of the polyethylene particles is preferably 300-800 μm, more preferably 350-750 μm, more preferably 400-700 μm, and most preferably 450-650 μm. After the average particle size of the polyethylene particles is optimized, the pore size of the implant obtained by sintering is more suitable. In the present invention, the average particle size of the polyethylene particles can be specifically 300 μm, 350 μm, 400 μm, 450 μm, 500 μm, 550 μm, 600 μm, 650 μm, 700 μm, 750 μm or 800 μm.

[0036] In the preparation method provided by the present invention, in step a), the polyethylene particles are spherical or nearly spherical, and the degree of spheroidization is preferably 40-100%, more preferably 50-100%, more preferably 60%-100%, and most preferably 80-100%. The polyethylene particles with a preferred degree of spheroidization have a more uniform pore size and a more uniform porosity after sintering. In the present invention, the degree of spheroidization of the polyethylene particles can be specifically 40%, 44%, 45%, 50%, 54%, 55%, 60%, 65%, 70%, 71%, 74%, 75%, 78%, 80%, 85%, 90%, 93%, 95% or 100%.

[0037] In the preparation method provided by the present invention, in step a), the spheroidization degree is defined as: the ratio of the equivalent diameter of the particle perimeter to the equivalent diameter of the particle area, which can be described by the following formula: Q = d1 / d a , where d1 represents the equivalent diameter of the particle's circumference. If the particle's circumference is l, then l=2πd1; d a Represents the area equivalent diameter of the particle. If the area of ​​the particle is A, then A=πd a ². The test method for spheroidization is: select the captured SEM image (the number of microparticles in the selected area is not less than 5), import it into Image-Pro PLUS software, and use the software calculation function to calculate the ratio of the equivalent diameter of the particle perimeter to the equivalent diameter of the particle area. The closer the equivalent diameter ratio is to 1, the higher the spheroidization degree. The higher the spheroidization degree, the more the stacking contact between particles will tend to be point contact, and the more uniform the pores formed.

[0038] In the preparation method provided by the present invention, in step b), the temperature and time of the sintering molding should be appropriately adjusted according to the melt index. When the sintering temperature is low, the fusion effect between particles is poor, the porosity is large but the mechanical strength is insufficient; when the sintering temperature is high, the fusion between particles is better, the porosity is low but the mechanical strength is high; at the same temperature, the longer the sintering time, the better the particle fusion and the smaller the porosity.

[0039] In the preparation method provided by the present invention, in step b), the sintering temperature is preferably 140-220°C, more preferably 150-210°C, more preferably 160-200°C, and most preferably 170-190°C. After the sintering temperature is optimized, the pore size and porosity of the implant are more suitable. In the present invention, the sintering temperature can be specifically 140°C, 145°C, 150°C, 155°C, 160°C, 165°C, 170°C, 175°C, 180°C, 185°C, 190°C, 195°C, 200°C, 205°C, 210°C, 215°C or 220°C.

[0040] In the preparation method provided by the present invention, in step b), the sintering time is preferably 3 to 15 minutes, more preferably 5 to 13 minutes, more preferably 6 to 12 minutes, and most preferably 7 to 11 minutes. After the sintering time is optimized, the pore size and porosity of the implant are more suitable. In the present invention, the sintering time can be specifically 3 minutes, 4 minutes, 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes, 10 minutes, 11 minutes, 12 minutes, 13 minutes, 14 minutes or 15 minutes.

[0041] In the preparation method provided by the present invention, in step b), the sintering equipment includes but is not limited to a vacuum drying oven, an electric heating tablet press or a flat vulcanizing machine. The equipment is preferably preheated before use. The preheating temperature is preferably 100-150°C, more preferably 120°C, and the preheating time is preferably 20-40 minutes, more preferably 30 minutes.

[0042] In the preparation method provided by the present invention, it is preferred to further include: in the process of preparing the porous polyethylene implant, functional modification is performed on it. In the present invention, the functional modification includes but is not limited to improving hydrophilicity to promote tissue growth and accelerate postoperative recovery; improving antibacterial ability to avoid infection in the short term after surgery; improving antioxidant ability to improve the long-term stability of the implant.

[0043] In the preparation method provided by the present invention, the functional modification method preferably includes sintering modification and / or surface modification. Wherein, the sintering modification refers to mixing the functional additives with the polyethylene particles obtained by underwater granulation in a certain proportion, adding them together to the mold for sintering molding; or immersing the finished porous polyethylene implant into a solution containing a certain proportion of functional additives, taking it out and then sintering it; or directly adding the functional additives to the finished porous polyethylene implant, oscillating it evenly and then sintering it, and the functional additives will melt and sinter into the pores of the porous polyethylene; the functional additives that can be used for sintering modification include but are not limited to one or more mixtures of nano-gold, nano-silver, nano-copper, nano-zinc oxide, nano-gallium oxide and bioglass. The surface modification method includes but is not limited to plasma treatment, acidification treatment or sandblasting treatment, and the main purpose is to improve the roughness, surface energy and hydrophilicity of the sample surface, and then immerse the surface-treated porous polyethylene in a polydopamine solution containing an antibacterial agent and / or an antioxidant to obtain a porous polyethylene containing a functional coating; the antibacterial agent includes but is not limited to one or more of triclosan, chitosan and antimicrobial peptides; the antioxidant includes but is not limited to one or more of vitamin E, tea polyphenols, proanthocyanidins and resveratrol.

[0044] In the preparation method provided by the present invention, when the sintering modification is performed, the added amount of the functional additive is preferably 1~5wt% of the mass of the porous polyethylene implant; when the surface modification is performed, the added amount of the antibacterial agent and the antioxidant is independently preferably 5~15wt% of the mass of the porous polyethylene implant.

[0045] In the preparation method provided by the present invention, the average pore size of the prepared porous polyethylene implant can be controllably adjusted within 30~300μm. At the same time, a porous polyethylene implant with a larger pore size can be prepared, so that its average pore size is preferably 60~300μm, more preferably 80~280μm, more preferably 100~260μm, and most preferably 120~240μm. A larger pore size is more suitable for cell and tissue growth, the tissue compatibility of the implant is improved, and immune rejection is less likely to occur. A pore size that is too small is not conducive to cell growth and the delivery of nutrients and the discharge of metabolic products. It is also easy for macrophages to be unable to grow into the holes to phagocytize residual bacteria and cause infection. A pore size that is too large will affect the long-term stability of the implant, and the low cell adhesion efficiency is not conducive to cell proliferation. In the present invention, the average pore size of the porous polyethylene implant can be 30μm, 40μm, 50μm, 60μm, 70μm, 80μm, 90μm, 100μm, 110μm, 120μm, 130μm, 140μm, 150μm, 160μm, 170μm, 180μm, 190μm, 200μm, 210μm, 220μm, 230μm, 240μm, 250μm, 260μm, 270μm, 280μm, 290μm or 300μm.

[0046] In the preparation method provided by the present invention, the porosity of the porous polyethylene implant obtained is preferably 20-60%, more preferably 30-60%, further preferably 35-60%, and most preferably 40-60%. The preferred porosity can maintain appropriate mechanical strength while allowing an appropriate amount of tissue to grow in, thereby promoting the stability of the implant. Too high a porosity is not conducive to cell adhesion, and the long-term stability of the implant will be affected, making the implant structure prone to damage; too low a porosity will hinder the ingrowth of tissue cells. In the present invention, the porosity of the porous polyethylene implant may specifically be 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39%, 40%, 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49%, 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59% or 60%.

[0047] The preparation method provided by the present invention first adopts an underwater granulation process to prepare large polyethylene particles with a certain particle size, and then sintering these large polyethylene particles in a mold. During the sintering process, the large polyethylene particles contact and bond with each other to form abundant and large three-dimensional holes. The method of the present invention can be used to prepare a porous polyethylene implant with a larger pore size. The larger pore size can promote the growth of tissue cells, making the implant less likely to shift, and can also promote the vascularization of the implant site, reducing the risk of infection. In addition, in the preferred technical solution provided by the present invention, the porous polyethylene implant can also be functionally modified to give it antibacterial, antioxidant and other biological functions, thereby further reducing the infection risk of the implant and increasing the service life of the implant.

[0048] For the purpose of greater clarity, the invention is described in detail through the following examples.

[0049] Example 1

[0050] A commercially available implant grade UHMWPE powder was selected, with a weight average molecular weight of 1500000 g / mol and a melt flow index of 0.5 g / 10 min (190°C, 21.6 kg); the UHMWPE powder, PEG2000 and Tween 80 were added to the twin-screw extruder of the underwater granulation system at a mass ratio of 90:5:5, and the extruder parameters were adjusted: screw speed 150 rpm, barrel rear section temperature 190°C, middle section temperature 200°C, front section temperature 210°C, die opening diameter 500 μm, cutting machine speed 700 rpm, circulating water temperature 80°C. After underwater granulation, nearly spherical UHWMPE microparticles with an average particle size of 500 μm were obtained, with an average spheroidization degree of 81%, and a microscopic morphology such as Figure 1 shown.

[0051] Weigh 10g of the above UHMWPE microparticles and pour them into the lower mold and flatten them, then cover them with an aluminum upper mold. Place the entire mold set on an electric heating tablet press preheated at 120℃ for 30min, ensuring that the upper mold and the upper mold of the tablet press are in non-pressure contact, and set the parameters: the insulation section temperature is 180℃, and the insulation section time is 10min. After the insulation sintering is completed, water cool to room temperature to obtain a porous polyethylene implant product with a microscopic morphology as shown in the figure. Figure 2 The pore parameters of the product were tested using a mercury intrusion instrument, and the average pore size of the product was 190μm and the porosity was 52%.

[0052] The porous polyethylene implant product was added to 10 mol / L concentrated sulfuric acid for acidification for 15 min, taken out and ultrasonically cleaned, then added to a polydopamine solution containing 10 wt% chitosan and 5 wt% vitamin E, stirred at room temperature for 48 h, taken out and ultrasonically cleaned and dried in turn, to obtain a porous polyethylene implant product containing a functional additive coating, the appearance of which is as follows: Figure 3shown.

[0053] Example 2

[0054] On the basis of Example 1, other process parameters were not adjusted, the die opening diameter was adjusted to 800 μm, and the cutting machine speed was adjusted to 300 rpm, to obtain nearly spherical UHMWPE microparticles with an average particle size of 800 μm and an average spheroidization degree of 78%.

[0055] After sintering the UHMWPE microparticles according to the method and conditions of Example 1, a porous polyethylene implant product with an average pore diameter of 250 μm and a porosity of 58% was obtained.

[0056] Example 3

[0057] On the basis of Example 1, other process parameters were not adjusted, the die opening diameter was adjusted to 300 μm, and the cutting machine speed was adjusted to 1200 rpm, to obtain nearly spherical UHMWPE microparticles with an average particle size of 300 μm and an average spheroidization degree of 75%.

[0058] After sintering the above UHMWPE microparticles according to the method and conditions of Example 1, a porous polyethylene implant product with an average pore diameter of 100 μm and a porosity of 30% was obtained.

[0059] Example 4

[0060] On the basis of Example 1, other process parameters were not adjusted, and the cutting machine speed was adjusted to 500 rpm, to obtain nearly spherical UHMWPE microparticles with an average particle size of 500 μm and an average spheroidization degree of 57%.

[0061] After sintering the UHMWPE microparticles according to the method and conditions of Example 1, a porous polyethylene implant product with an average pore diameter of 170 μm and a porosity of 38% was obtained.

[0062] Example 5

[0063] On the basis of Example 1, other process parameters were not adjusted, and the cutting machine speed was adjusted to 300 rpm, and nearly spherical UHMWPE microparticles with an average particle size of 500 μm and an average spheroidization degree of 44% were obtained.

[0064] After sintering the UHMWPE microparticles according to the method and conditions of Example 1, a porous polyethylene implant product with an average pore diameter of 150 μm and a porosity of 31% was obtained.

[0065] Example 6

[0066] On the basis of Example 1, other process parameters were not adjusted, and the cutting machine speed was adjusted to 1000 rpm to obtain ellipsoidal UHMWPE microparticles with an average particle size of 500 μm and an average spheroidization degree of 61%.

[0067] After sintering the UHMWPE microparticles according to the method and conditions of Example 1, a porous polyethylene implant product with an average pore diameter of 180 μm and a porosity of 40% was obtained.

[0068] Example 7

[0069] On the basis of Example 1, other process parameters were not adjusted, and the cutting machine speed was adjusted to 1200 rpm to obtain ellipsoidal UHMWPE microparticles with an average particle size of 500 μm and an average spheroidization degree of 52%.

[0070] After sintering the UHMWPE microparticles according to the method and conditions of Example 1, a porous polyethylene implant product with an average pore diameter of 150 μm and a porosity of 35% was obtained.

[0071] Example 8

[0072] On the basis of Example 1, other process parameters were not adjusted, and the die opening diameter was adjusted to 300 μm, and ellipsoidal UHMWPE microparticles with an average particle size of 300 μm were obtained, and the average spheroidization degree was 62%.

[0073] After sintering the UHMWPE microparticles according to the method and conditions of Example 1, a porous polyethylene implant product with an average pore diameter of 90 μm and a porosity of 28% was obtained.

[0074] Example 9

[0075] On the basis of Example 1, other process parameters were not adjusted, and the die opening diameter was adjusted to 800 μm, to obtain ellipsoidal UHMWPE microparticles with an average particle size of 800 μm and an average spheroidization degree of 58%.

[0076] After sintering the UHMWPE microparticles according to the method and conditions of Example 1, a porous polyethylene implant product with an average pore diameter of 220 μm and a porosity of 47% was obtained.

[0077] Example 10

[0078] A commercially available implantable HDPE powder was selected, with a weight average molecular weight of 250,000 g / mol and a melt flow index of 30 g / 10 min (190°C, 21.6 kg); the HDPE powder, PEG2000 and Tween 80 were added to the twin-screw extruder of the underwater granulation system at a mass ratio of 95:2.5:2.5, and the extruder parameters were adjusted: screw speed 200 rpm, barrel rear section temperature 190°C, middle section temperature 200°C, front section temperature 210°C, die opening diameter 500 μm, cutter speed 500 rpm, circulating water temperature: 80°C. After underwater granulation, nearly spherical HDPE microparticles with an average particle size of 500 μm were obtained, and the average spheroidization degree was 90%.

[0079] Weigh 10g of the above HDPE microparticles and 0.2g of medical nanosilver particles, mix them evenly, pour them into the lower mold and flatten them, and cover them with an aluminum upper mold. Place the entire set of molds on an electric heating tablet press preheated at 120°C for 30 minutes to ensure that the upper mold is in non-pressure contact with the upper mold of the tablet press, and set the parameters: the insulation section temperature is 180°C, and the insulation section time is 5 minutes. After the insulation sintering is completed, water cool to room temperature to obtain a porous polyethylene implant product. The product was tested for pore parameters using a mercury intrusion instrument. The average pore size of the product was 200μm and the porosity was 47%.

[0080] Embodiment 11

[0081] On the basis of Example 10, other process parameters were not adjusted, and a commercially available implant grade HDPE powder was selected, whose weight average molecular weight was 400000 g / mol and melt flow index was 10 g / 10 min (190°C, 21.6 kg); cylindrical HDPE microparticles with an average particle size of 500 μm and an average spheroidization degree of 54% were obtained through an underwater granulation process.

[0082] After sintering the HDPE microparticles according to the method and conditions of Example 10, a porous polyethylene implant product with an average pore diameter of 90 μm and a porosity of 31% was obtained.

[0083] Example 12

[0084] On the basis of Example 10, other process parameters were not adjusted, and a commercially available implant-grade HDPE powder was selected, whose weight-average molecular weight was 150,000 g / mol and melt flow index was 50 g / 10 min (190°C, 21.6 kg); through an underwater granulation process, nearly spherical HDPE microparticles with an average particle size of 500 μm were obtained, and the average degree of spheroidization was 93%.

[0085] After sintering the HDPE microparticles according to the method and conditions of Example 10, a porous polyethylene implant product with an average pore diameter of 40 μm and a porosity of 26% was obtained.

[0086] Example 13

[0087] On the basis of Example 10, other process parameters were not adjusted, and the holding time of the tablet press was set to 10 min, to obtain a porous polyethylene implant product with an average pore diameter of 140 μm and a porosity of 36%.

[0088] Embodiment 14

[0089] On the basis of Example 10, other process parameters were not adjusted, and the holding time of the tablet press was set to 3 minutes to obtain a porous polyethylene implant product with an average pore diameter of 220 μm and a porosity of 49%.

[0090] Embodiment 15

[0091] On the basis of Example 10, other process parameters were not adjusted, and the temperature of the insulation section of the tablet press was set to 220° C. to obtain a porous polyethylene implant product with an average pore diameter of 80 μm and a porosity of 28%.

[0092] Example 16

[0093] On the basis of Example 10, other process parameters were not adjusted, and the temperature of the insulation section of the tablet press was set to 140° C. to obtain a porous polyethylene implant product with an average pore diameter of 260 μm and a porosity of 58%.

[0094] Embodiment 17

[0095] On the basis of Example 10, HDPE powder, PEG2000 and Tween 80 were added to the twin-screw extruder of the underwater granulation system in a mass ratio of 100:0:0, and other processes were not adjusted to obtain nearly spherical HDPE microparticles with an average particle size of 500 μm and an average spheroidization degree of 78%.

[0096] Embodiment 18

[0097] After sintering the HDPE microparticles according to the method and conditions of Example 10, a porous polyethylene implant product with an average pore diameter of 170 μm and a porosity of 43% was obtained.

[0098] On the basis of Example 10, HDPE powder, PEG2000 and Tween 80 were added to the twin-screw extruder of the underwater granulation system in a mass ratio of 90:5:5, and other processes were not adjusted to obtain nearly spherical HDPE microparticles with an average particle size of 500 μm and an average spheroidization degree of 96%.

[0099] After sintering the HDPE microparticles according to the method and conditions of Example 10, a porous polyethylene implant product with an average pore size of 220 μm and a porosity of 54% was obtained.

[0100] Embodiment 19

[0101] On the basis of Example 10, HDPE powder, PEG2000 and Tween 80 were added to the twin-screw extruder of the underwater granulation system in a mass ratio of 95:1:4, and other processes were not adjusted to obtain nearly spherical HDPE microparticles with an average particle size of 500 μm and an average spheroidization degree of 77%.

[0102] After sintering the HDPE microparticles according to the method and conditions of Example 10, a porous polyethylene implant product with an average pore size of 220 μm and a porosity of 52% was obtained.

[0103] Embodiment 20

[0104] On the basis of Example 10, HDPE powder, PEG2000 and Tween 80 were added to the twin-screw extruder of the underwater granulation system in a mass ratio of 95:4:1, and other processes were not adjusted to obtain nearly spherical HDPE microparticles with an average particle size of 500 μm and an average spheroidization degree of 78%.

[0105] After sintering the HDPE microparticles according to the method and conditions of Example 10, a porous polyethylene implant product with an average pore size of 220 μm and a porosity of 53% was obtained.

[0106] Through Examples 1, 4 to 7, it can be seen that under the same conditions, as the cutting speed increases, the degree of spheroidization first increases and then decreases, and the average pore size and porosity of the porous polyethylene implant product finally prepared also first increase and then decrease. The degree of spheroidization can be controlled as needed to adjust the uniformity of its pore size, and the average pore size and porosity of the prepared porous polyethylene implant product can be further adjusted and controlled.

[0107] Through Examples 1, 9 and 10, it can be seen that, under the same conditions, as the die opening diameter increases, the average pore size increases accordingly.

[0108] Through Examples 10, 17-18, it can be seen that under the same conditions, as the amount of PEG2000 and Tween 80 increases, the degree of spheroidization gradually increases, and the average pore size and porosity of the porous polyethylene implant product finally prepared also gradually increase. By increasing the surfactant and plasticizer, the degree of spheroidization can be improved, and the average pore size and porosity of the porous polyethylene implant product prepared can be adjusted and controlled.

[0109] Through Examples 10, 19, and 20, it can be seen that under the same conditions, when the total mass ratio of the surfactant and the plasticizer remains unchanged, the ratio of the surfactant and the plasticizer changes, there is no obvious difference in the spheroidization degree, and there is no obvious difference in the average pore size and porosity of the porous polyethylene implant products.

[0110] Through Examples 10-12, it can be seen that under the same conditions, as the molecular weight increases, the spheroidization degree gradually decreases, and the average pore size and porosity of the porous polyethylene implant product finally prepared gradually increase. By adjusting the molecular weight of the polyethylene used, the spheroidization degree can be adjusted and controlled, and the average pore size and porosity of the porous polyethylene implant product prepared can be adjusted and controlled.

[0111] Through Examples 10, 13, and 14, it can be seen that under the same conditions, as the holding time of the tablet press increases, the average pore size and porosity of the porous polyethylene implant product finally prepared gradually decrease. By adjusting the holding time of the tablet press, the average pore size and porosity of the porous polyethylene implant product prepared can be adjusted and controlled.

[0112] Through Examples 10, 15, and 16, it can be seen that under the same conditions, as the temperature of the tablet press insulation section increases, at the same insulation time, the average pore size and porosity of the porous polyethylene implant product finally prepared gradually decrease. By adjusting the tablet press insulation temperature, the average pore size and porosity of the prepared porous polyethylene implant product can be adjusted and controlled.

[0113] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a porous polyethylene implant, characterized in that: The following steps are involved: a) melt-extrude the polyethylene and then perform underwater granulation to obtain polyethylene particles with an average particle size of 300-800 μm; b) filling the polyethylene particles into a mold, sintering and cooling to obtain a porous polyethylene implant.

2. The preparation method according to claim 1, characterized in that: In step a), the polyethylene has a melt flow index of 0.5-50 g / 10 min under test conditions of 190° C. and 21.6 kg; and a weight average molecular weight of 150,000-1,500,000 g / mol.

3. The preparation method according to claim 1, characterized in that: In step a), a plasticizer and / or a surfactant is also added during the melting process.

4. The preparation method according to claim 3, characterized in that: In step a), the plasticizer is one or more of PEG400, PEG2000 and PEG4000; the surfactant is one or more of Span 40, Tween 40 and Tween 80.

5. The preparation method according to claim 3, characterized in that: In step a), the plasticizer accounts for 0-5% of the total mass of polyethylene, plasticizer and surfactant; the surfactant accounts for 0-5% of the total mass of polyethylene, plasticizer and surfactant.

6. The preparation method according to claim 1, characterized in that: In step a), the melt extrusion is carried out in a twin-screw extruder, the die opening diameter of the twin-screw extruder is 300-800 μm; the melt extruded melt is cut and granulated underwater, and the cutting machine speed is 300-1200 rpm.

7. The preparation method according to claim 6, characterized in that: In step a), the screw speed of the twin-screw extruder is 100-300 rpm, and the barrel temperature is 180-220° C.; the water temperature of the melt during underwater cutting and granulation is 60-90° C.

8. The preparation method according to claim 1, characterized in that: In step a), the polyethylene particles have a spheroidization degree of 40-100%.

9. The preparation method according to claim 1, characterized in that: In step b), the sintering temperature is 140-220° C. and the sintering time is 3-15 min.

10. The preparation method according to claim 1, characterized in that: Also includes: During the preparation of the porous polyethylene implant, it is functionally modified.

11. The preparation method according to claim 10, characterized in that: The functional modification methods include sintering modification and / or surface modification.

Citation Information

Patent Citations

  • Manufacturing method of artificial sclerite shaping implant with polyvinyl plastics

    CN101161294A

  • Preparation method of self-reinforced polyethylene blend for full-joint implantation

    CN102167860A

  • Material combining porous ultrahigh molecular weight polyethylene and bionic cartilage and manufacturing technology

    CN103418032A

  • Ultrahigh molecular weight polyethylene composite material for fusible body processing of artificial joint

    CN103751849A

  • Porous implants for dentistry and surgery and manufacturing method thereof