Method for preparing sodium-ion battery hard carbon negative electrode material through porous carbon modification and application of sodium-ion battery hard carbon negative electrode material

By ball milling, the asphalt is adsorbed to the porous carbon orifice and carbonized at high temperature, transforming the open pore into a closed pore structure, solving the problems of low capacity of the hard carbon negative electrode material platform of sodium ion battery and poor efficiency for the first time, and achieving high-efficiency sodium ion battery Preparation of negative electrode materials, suitable for large-scale industrial production.

CN119018878AInactive Publication Date: 2024-11-26BEIJING UNIV OF CHEM TECH

Patent Information

Application Number
CN202411153258.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing sodium ion battery hard carbon anode material platform has low capacity and poor first-time Coulomb efficiency. The existing preparation process is complex and costly, making it difficult to achieve large-scale industrial production.

Method used

Asphalt and porous carbon are used as carbon sources, and the asphalt is adsorbed at the porous carbon pores by ball milling and carbonized at high temperatures, transforming the open-porous structure into a closed-porous structure, thereby increasing the platform capacity.

Benefits of technology

It improves the efficiency and reversible capacity of the first Coulomb, has a simple preparation process, rich raw materials, low price, is suitable for large-scale industrial production, and is environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119018878A_ABST
    Figure CN119018878A_ABST
Patent Text Reader

Abstract

The invention relates to the field of sodium-ion battery hard carbon negative electrode materials, in particular to the technical field of a method for preparing a sodium-ion battery hard carbon negative electrode material through porous carbon modification. Asphalt and porous carbon are used as carbon sources, the asphalt and the porous carbon are uniformly mixed through a simple ball milling method, so that the asphalt is adsorbed at the opening of the porous carbon, and further high-temperature carbonization is performed to convert the opening structure on the surface of the porous carbon into a closed-pore structure, so that the platform capacity of the porous carbon is improved. The preparation method has the characteristics of wide raw material asphalt source, low price, simple preparation process method, environmental friendliness and the like, and is suitable for large-scale industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of hard carbon negative electrode materials for sodium ion batteries, and in particular to a method for preparing hard carbon negative electrode materials for sodium ion batteries by modifying porous carbon and application thereof. Background Art

[0002] Among the many new energy technologies, rechargeable batteries have the characteristics of high energy density and large capacity, and are one of the energy storage technologies that best meet our daily needs. However, lithium resources are scarce and unevenly distributed, and the cost is high, so lithium-ion batteries are not suitable for large-scale energy storage.

[0003] Sodium-ion batteries are considered to be the best alternative to lithium-ion batteries due to their abundant sodium reserves, low cost, and physical and chemical properties similar to those of lithium-ion batteries. Among them, hard carbon is considered to be the most commercially promising negative electrode material for sodium-ion batteries. However, hard carbon as a negative electrode for sodium-ion batteries has disadvantages such as low platform capacity and poor first coulombic efficiency. The charge and discharge curve of hard carbon negative electrode materials usually consists of a low potential platform region and a high potential slope region. Improving the sodium storage capacity of the platform region by microstructural regulation is an important research direction for hard carbon negative electrode materials for sodium-ion batteries. Patent CN 117712355 A introduces carbon source gas into porous carbon materials during the carbonization process, and performs chemical vapor deposition on the surface of the porous material to obtain negative electrode materials. However, the CVD process is too complicated and requires special equipment. In addition, the amount of coating is difficult to accurately control, and the industrialization cost is high and the safety requirements are stringent. In patent CN 118324122 A, asphalt or tar is mixed with biochar, and hard carbon negative electrode materials for sodium-ion batteries are obtained after high-temperature carbonization. However, the specific surface area of ​​biochar is very low and there are few surface openings. After mixed carbonization, the closed-pore structure of the biochar itself still provides the main capacity, rather than the part of the structure that changes from open pores to closed pores after coating. The role of asphalt or coke here is mainly to improve the conductivity of biochar. Summary of the invention

[0004] The present invention provides a method for preparing a hard carbon negative electrode material for a sodium ion battery by modifying porous carbon according to the problem to be solved. Asphalt and porous carbon are used as carbon sources, and the asphalt and porous carbon are evenly mixed by a simple ball milling method, so that the asphalt is adsorbed on the openings of the porous carbon, and further high-temperature carbonization is performed to convert the open-pore structure on the surface of the porous carbon into a closed-pore structure, thereby increasing the platform capacity of the porous carbon. The preparation process has the advantages of abundant raw material asphalt sources, low price, simple preparation process, and environmental friendliness, and is suitable for large-scale industrial production.

[0005] The steps of preparing a hard carbon negative electrode material for a sodium ion battery by modifying porous carbon are as follows:

[0006] Step (1) weighing a certain mass ratio of asphalt and porous carbon into a ball mill for a period of time to form a precursor;

[0007] Step (2) subjecting the precursor obtained in step (1) to high-temperature carbonization treatment in an inert atmosphere, wherein the carbonization temperature is 1300° C.-1600° C., and after high-temperature treatment, a hard carbon negative electrode material having a rich closed-pore structure is obtained.

[0008] Preferably: the asphalt in step (1) is one or more of medium-temperature coal asphalt, high-temperature coal asphalt, petroleum asphalt, and mesophase asphalt; the porous carbon has a specific surface area of ​​800m 2 g -1 -3500m 2 g -1 , one or more porous carbons with a micropore content greater than 75%, the mass ratio of asphalt to porous carbon is 1:(1-5), and the ball milling time is 30-180min.

[0009] Preferably, the inert atmosphere in step (2) is argon, and the heating rate is 2-5°C / min.

[0010] Beneficial effects of the present invention

[0011] The negative electrode material provided by the present invention uses a simple ball milling method to adsorb asphalt on the pores of porous carbon, and further high-temperature carbonization transforms the open-pore structure on the surface of the porous carbon into a closed-pore structure, reducing structural defects and improving the regularity of the carbon layer, thereby improving the first coulombic efficiency and reversible capacity. The preparation process has the advantages of abundant raw material asphalt sources, low price, simple preparation process, and environmental friendliness, and is suitable for large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1 It is a scanning electron microscope image of the carbonized sample of Example 4 of the present invention.

[0013] Figure 2 It is the charge and discharge curve of the samples of comparative example 1 and embodiment 4 of the present invention.

[0014] The present invention is further described below by way of specific embodiments, but is not intended to limit the present invention.

[0015] Embodiment 1:

[0016] Step (1) Weigh 1 g of mesophase pitch and 5 g of commercial activated carbon 1, whose specific surface area is 1959.21 m 2 / g, micropore content 85.2%, put into a ball mill for 30 minutes to form a precursor;

[0017] Step (2) subjecting the precursor obtained in step (1) to high-temperature carbonization treatment under an inert atmosphere, the carbonization temperature being 1300° C., and obtaining a hard carbon negative electrode material after high-temperature treatment.

[0018] The electrochemical performance test results show that the electrode material has a -1 The discharge capacity at the current density can reach 274 mAh g -1 .

[0019] Embodiment 2:

[0020] Step (1) Weigh 1 g of mesophase pitch and 5 g of commercial activated carbon 1, whose specific surface area is 1959.21 m 2 / g, micropore content 85.2%, put into a ball mill for 180min to form a precursor;

[0021] Step (2) subjecting the precursor obtained in step (1) to high-temperature carbonization treatment under an inert atmosphere, the carbonization temperature being 1300° C., and obtaining a hard carbon negative electrode material after high-temperature treatment.

[0022] The electrochemical performance test results show that the electrode material has a -1 The discharge capacity at the current density can reach 214 mAh g -1 .

[0023] Embodiment 3:

[0024] Step (1) Weigh 1 g of mesophase pitch and 1 g of commercial activated carbon 1, whose specific surface area is 1959.21 m 2 / g, micropore content 85.2%, put into a ball mill for 30 minutes to form a precursor;

[0025] Step (2) subjecting the precursor obtained in step (1) to high-temperature carbonization treatment under an inert atmosphere, the carbonization temperature being 1300° C., and obtaining a hard carbon negative electrode material after high-temperature treatment.

[0026] The electrochemical performance test results show that the electrode material has a -1 The discharge capacity at the current density can reach 290mAhg -1 .

[0027] Embodiment 4:

[0028] Step (1) Weigh 1 g of mesophase pitch and 3 g of commercial activated carbon 2, whose specific surface area is 2428.42 m 2 / g, micropore content 79.8%, put into a ball mill for 30 minutes to form a precursor;

[0029] Step (2) subjecting the precursor obtained in step (1) to high-temperature carbonization treatment under an inert atmosphere, the carbonization temperature being 1300° C., and obtaining a hard carbon negative electrode material after high-temperature treatment.

[0030] The electrochemical performance test results show that the electrode material has a-1 The discharge capacity at the current density can reach 324mAhg -1 .

[0031] Embodiment 5:

[0032] Step (1) Weigh 1 g of mesophase pitch and 3 g of commercial activated carbon 1, whose specific surface area is 1959.21 m 2 / g, micropore content 85.2%, put into a ball mill for 30 minutes to form a precursor;

[0033] Step (2) subjecting the precursor obtained in step (1) to high-temperature carbonization treatment under an inert atmosphere, the carbonization temperature being 1500° C., and obtaining a hard carbon negative electrode material after high-temperature treatment.

[0034] The electrochemical performance test results show that the electrode material has a -1 The discharge capacity at the current density can reach 304mAhg -1 .

[0035] Embodiment 6:

[0036] Step (1) Weigh 1 g of mesophase pitch and 3 g of commercial activated carbon 1, whose specific surface area is 1959.21 m 2 / g, micropore content 85.2%, put into a ball mill for 30 minutes to form a precursor;

[0037] Step (2) subjecting the precursor obtained in step (1) to high-temperature carbonization treatment under an inert atmosphere, the carbonization temperature being 1600° C., and obtaining a hard carbon negative electrode material after high-temperature treatment.

[0038] The electrochemical performance test results show that the electrode material has a -1 The discharge capacity at the current density can reach 280mAhg -1 .

[0039] Embodiment 7:

[0040] Step (1) Weigh 1 g of petroleum asphalt and 4 g of commercial activated carbon 2, whose specific surface area is 2428.42 m 2 / g, micropore content 79.8%, put into a ball mill for 30 minutes to form a precursor;

[0041] Step (2) subjecting the precursor obtained in step (1) to high-temperature carbonization treatment under an inert atmosphere, the carbonization temperature being 1500° C., and obtaining a hard carbon negative electrode material after high-temperature treatment.

[0042] The electrochemical performance test results show that the electrode material has a -1The discharge capacity at the current density can reach 285 mAh g -1 .

[0043] Embodiment 8:

[0044] Step (1) Weigh 1 g of medium-temperature coal tar and 3 g of commercial activated carbon 2, whose specific surface area is 2428.42 m 2 / g, micropore content 79.8%, put into a ball mill for 120min to form a precursor;

[0045] Step (2) subjecting the precursor obtained in step (1) to high-temperature carbonization treatment under an inert atmosphere, the carbonization temperature being 1300° C., and obtaining a hard carbon negative electrode material after high-temperature treatment.

[0046] The electrochemical performance test results show that the electrode material has a -1 The discharge capacity at the current density can reach 276 mAh g -1 .

[0047] Comparative Example 1: Commercial activated carbon 2, with a specific surface area of ​​2428.42 m 2 / g, micropore content of 79.8%, after ball milling for 30min, high temperature carbonization at 1300℃ was directly carried out in an inert atmosphere. -1 The discharge capacity at the current density is only 126 mAh g -1 , and there is no platform capacity.

[0048] The preferred embodiments of the present invention have been specifically described above, but the present invention is not limited to the embodiments. Those skilled in the art may make various equivalent modifications or substitutions without violating the spirit of the present invention. These equivalent modifications or substitutions are all included in the scope defined by the claims of this application.

Claims

1. A method for preparing a hard carbon negative electrode material for a sodium ion battery by modifying porous carbon, the steps of which are as follows: Step (1) weighing a certain mass ratio of asphalt and porous carbon into a ball mill for a period of time to form a precursor; Step (2) subjecting the precursor obtained in step (1) to high-temperature carbonization treatment in an inert atmosphere, wherein the carbonization temperature is 1300° C.-1600° C., and after high-temperature treatment, a hard carbon negative electrode material having a rich closed-pore structure is obtained.

2. The preparation method according to claim 1, wherein the asphalt in step (1) is one or more of medium-temperature coal asphalt, high-temperature coal asphalt, petroleum asphalt, and mesophase asphalt; the porous carbon has a specific surface area of ​​800 m 2 g -1 -3500m 2 g -1 , one or more porous carbons with a micropore content greater than 75%, the mass ratio of asphalt to porous carbon is 1:(1-5), and the ball milling time is 30-180min.

3. The preparation method according to claim 1, wherein the inert atmosphere in step (2) is argon and the heating rate is 2-5°C / min.

4. The preparation method according to claim 1, wherein the pitch-modified activated carbon is characterized in that the pitch-modified activated carbon contains the preparation method according to any one of claims 1 to 3.

5. The asphalt-modified activated carbon prepared according to any one of claims 1 to 3 is used as a negative electrode material for sodium ion batteries.

Citation Information

Patent Citations

  • Lignin-based hard carbon material, preparation method thereof and application of lignin-based hard carbon material in sodium-ion battery

    CN117902577A

  • Biomass hard carbon material as well as preparation method and application thereof

    CN118062823A

  • Coal-based hard carbon negative electrode material, preparation method thereof and sodium ion battery

    CN118183739A

  • Preparation method of coal-based carbon material for sodium ion battery negative electrode

    CN118343755A

  • Method for preparing hard carbon material by compounding coal / biomass / asphalt, hard carbon material and application

    CN118419903A

Cited By

  • Porous carbon, silicon carbon negative electrode material, preparation method, pole piece and battery

    CN119706798A

  • Ultrathin carbon layer coated petroleum-based porous hard carbon microsphere negative electrode material and preparation method and application thereof