Preparation method of hollow ultramicro-spheres with adjustable components and thickness
By reacting silica with zinc-based coordination polymer at high temperature to form hollow zinc silicate and silica-coated zinc silicate hollow sphere composites, the existing zinc silicate materials are solved by single function and poor biocompatibility. The problem of this paper realizes the preparation of hollow ultramicrospheres with adjustable components and thicknesses, expanding its application in multiple fields.
Patent Information
- Application Number
- CN202411127337.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-16
AI Technical Summary
The zinc silicate materials prepared in the prior art have problems of single function, poor biocompatibility and modifyability.
The coating method is used to react silica with zinc-based coordination polymer at high temperature, and gradually decompose to form a hollow zinc silicate-coated hollow sphere composite with hollow structure, and adjust the zinc-based coordination. The polymer surface coated with silica thickness, hollow ultramicrospheres with adjustable components and thickness are prepared.
It realizes simple operation without reducing atmosphere, the product has good morphology, adjustable components, good biocompatibility and versatility, and expands the silicate in the fields of catalysis, energy storage, chemical reactors and biomedicine. application.
Smart Images

Figure CN119018904A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the preparation of hollow ultramicrospheres, and in particular to a method for preparing hollow ultramicrospheres with adjustable components and thickness. Background Art
[0002] Silicon dioxide is a common inorganic compound, which has important uses in our daily life, production and scientific research. Silicon dioxide has stable chemical properties, high temperature resistance, corrosion resistance, high insulation, unique optical properties and good biocompatibility. It is an important material for manufacturing glass, optical fibers, optical instruments, refractory materials and scientific research.
[0003] Zinc silicate has high thermal stability, chemical stability, good weather resistance and corrosion resistance, and is widely used in ceramics, coatings, rubber thickeners and biomedicine. There are already some methods for preparing zinc silicate with different structures, such as:
[0004] Publication No. CN118108228A The present invention provides a method for preparing clustered spherical zinc silicate microspheres. The method uses a surfactant as a template, a soluble zinc salt solution as a zinc source, and an organic silicon or a soluble silicate solution as a silicon source. Under alkaline conditions, a one-step hydrothermal reaction is performed to obtain clustered spherical zinc silicate microspheres with uniform size and complete assembly.
[0005] A method for preparing zinc silicate flower-shaped porous microspheres disclosed in a Chinese patent document with publication number CN117003253A comprises the following steps: (1) adding a surfactant to deionized water and fully dissolving it; (2) slowly dropping a silicon source into (1) and allowing it to react fully; (3) slowly dropping a dissolved zinc source solution into (2) and stirring it evenly; (4) adjusting the pH of the solution to a strong acid and stirring it evenly; (5) transferring the solution (4) to a hydrothermal reactor and obtaining Zn2SiO4 flower-shaped porous microspheres through a hydrothermal reaction.
[0006] A method for preparing a nano-flaky zinc silicate composite adsorbent using iron tailings is disclosed in a Chinese patent document with publication number CN109824055A. The method comprises the following steps: mixing the iron tailings, sodium salt and ethanol into a paste, then ball milling for 0.5 to 2 hours to obtain a dry powder, passing the dry powder through a 300-mesh sieve to obtain a powder, then adding the powder to water, stirring and adding zinc salt, vigorously stirring for 20 to 40 minutes to dissolve the zinc salt, continuing to stir and react for 2 hours to 6 hours to obtain a suspension, transferring the suspension to a hydrothermal reactor, and reacting at 120 to 220 degrees Celsius. The method comprises the following steps: preparing the composite material by mixing the raw materials for 8 to 72 hours, cooling naturally to room temperature, centrifuging, washing, drying, grinding and sieving to obtain an off-white lamellar zinc silicate composite material; adding 0.1 to 1.5 mol of sodium salt and 45 to 75 mL of ethanol to every 100 g of iron tailings; the mass of the powder is 1 to 10% of the suspension; the theoretical silicon-zinc molar ratio before the reaction is 5:1 to 1:1; the mass percentage of SiO-2 in the iron tailings is 65 to 80%; the sodium salt is one or both of sodium acetate and sodium silicate; the zinc salt is one or more of zinc sulfate, zinc chloride, zinc nitrate and zinc acetate.
[0007] Although these methods obtain zinc silicate with different structures, the zinc silicate prepared by these methods still has the disadvantages of single function, poor biocompatibility and modifiability. Summary of the invention
[0008] The present invention adopts a coating method to make silicon dioxide react with a zinc-based coordination polymer at high temperature, the coordination polymer gradually decomposes at high temperature, and the part in contact with silicon dioxide reacts to generate zinc silicate, thereby obtaining a hollow zinc silicate and silicon dioxide-coated zinc silicate hollow sphere composite (Zn2SiO4@SiO2). By adjusting the thickness of silicon dioxide coated on the surface of the zinc-based coordination polymer, the thickness of the silicon shell of Zn2SiO4@SiO2 can be adjusted. The method has the advantages of simple operation, no need for reducing atmosphere, and the obtained product has the advantages of good morphology, adjustable components, good biocompatibility, multifunctionality, etc.
[0009] The present invention provides a method for preparing hollow ultramicrospheres with adjustable components and thickness, and the specific steps are as follows:
[0010] (1) dissolving zinc nitrate hexahydrate, folic acid and polyvinyl pyrrolidone in a mixed solvent of N,N-dimethylformamide and anhydrous ethanol to obtain a mixed solution;
[0011] (2) stirring the mixed solution uniformly, transferring it into a reaction kettle, and placing it into an oven for reaction to obtain a zinc-based coordination polymer;
[0012] (3) washing the zinc-based coordination polymer with deionized water and anhydrous ethanol alternately and then vacuum drying to obtain ZnCPs;
[0013] (4) ultrasonically dispersing the ZnCPs and hexadecyltrimethylammonium bromide in a mixed solution of deionized water and anhydrous ethanol, stirring evenly for the first time after ultrasonic dispersion, adding an ethanol solution containing aqueous ammonia, stirring evenly for the second time, respectively adding tetraethyl orthosilicate, and then maintaining the mixture at room temperature for a third stirring reaction;
[0014] (5) The obtained product is collected by centrifugation, and washed alternately with deionized water and anhydrous ethanol, and then placed in a vacuum drying oven to obtain a zinc-based coordination polymer core-shell structure with different silica shell thicknesses. Finally, it is placed in a muffle furnace for calcination to obtain a zinc silicate with a hollow structure or a silicon dioxide-coated zinc silicate hollow sphere composite with different shell thicknesses.
[0015] Preferably, in step (1), the amount of zinc nitrate hexahydrate is 2 mmol, folic acid is 0.1 g, polyvinyl pyrrolidone is 0.1 g, the molecular weight of polyvinyl pyrrolidone is 1300000, and the volumes of N,N-dimethylformamide and anhydrous ethanol are 24 mL and 8 mL respectively.
[0016] Preferably, in step (2), the stirring time is 30 min to 60 min, and the reaction condition is 100° C. for 24 h.
[0017] Preferably, in step (3), the number of alternating washings is 3 times, the temperature of the drying treatment is 60° C., and the drying time is 24 hours.
[0018] Preferably, in step (4), the amount of ZnCPs used is 0.1 g, hexadecyltrimethylammonium bromide is 0.05 g, deionized water is 3 mL, and anhydrous ethanol is 20 mL. The mixture is ultrasonically dispersed for 1 h, stirred for the first time for 20 min, and the water temperature of the ultrasound is controlled between 20 and 40 °C.
[0019] Preferably, in step (4), the volumes of ammonia water and ethanol in the ammonia ethanol solution are 400 μL and 20 mL respectively, the second stirring time is 5 min, the amount of tetraethyl orthosilicate used is 200 μL to 1200 μL, and the third stirring time is 24 h.
[0020] Preferably, in step (5), the drying temperature is 60° C. and the drying time is 24 hours.
[0021] Preferably, in step (5), the calcination temperature is 1000° C., the calcination time is 4 h, and the heating rate is 1° C. / min.
[0022] Preferably, the hollow ultramicrospheres have a large specific surface area and a reaction cavity. The hollow ultramicrospheres are specifically zinc silicate or silicon dioxide-coated zinc silicate hollow sphere composites with a hollow structure. The thickness of silicon dioxide in the silicon dioxide-coated zinc silicate hollow sphere composite can be adjusted.
[0023] Preferably, the hollow ultramicrospheres can be used to adsorb heavy metal ions and organic pollutants in industrial wastewater, and to catalyze the reduction of gaseous pollutants such as NO, CO and CO; they can also be used in energy storage, chemical reactors, biomedicine, drug transport, sensing, optoelectronic devices, information encryption, drug loading and bioimaging.
[0024] Beneficial effects of the present invention:
[0025] The preparation process provided by the present invention is to coat ZnCPs with SiO2 and then perform high-temperature calcination, wherein the zinc-based coordination polymer gradually decomposes at high temperature, and the part in contact with silicon dioxide reacts at high temperature to generate zinc silicate, and by adjusting the thickness of the zinc-based coordination polymer coated with silicon dioxide, zinc silicate hollow spheres and silicon dioxide-coated zinc silicate hollow sphere composites with different thicknesses can be obtained, wherein the silicon shell thickness of the silicon dioxide-coated zinc silicate hollow sphere composite is adjustable, and has good biocompatibility.
[0026] This synthesis method uses coordination polymers as templates and precursors, reduces energy consumption, and also obtains hollow structure zinc silicate and silicon dioxide-coated zinc silicate composites, providing a new method for preparing new structure silicates and their composite materials, and expanding the application of silicates in various fields. This structure has broad application prospects in catalysis, energy storage, chemical reactors, biomedicine and other fields due to its advantages such as large specific surface area, low density, large pore volume and unique reaction cavity. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is the SEM image of ZnCPs prepared in Example 1 of the present invention.
[0028] Figure 2 This is the SEM image of ZnCPs@SiO2 prepared in Example 1 of the present invention.
[0029] Figure 3 This is the SEM image of Zn2SiO4 prepared in Example 1 of the present invention.
[0030] Figure 4 This is the TEM image of ZnCPs prepared in Example 1 of the present invention.
[0031] Figure 5 This is the TEM image of ZnCPs@SiO2 prepared in Example 1 of the present invention.
[0032] Figure 6 This is the TEM image of Zn2SiO4 prepared in Example 1 of the present invention.
[0033] Figure 7 This is the SEM image of ZnCPs@SiO2 prepared in Example 4 of the present invention.
[0034] Figure 8 This is a TEM image of the Zn2SiO4@SiO2 composite prepared in Example 4 of the present invention.
[0035] Fig. 9 The XRD diagrams of the zinc-based coordination polymer and the silicon dioxide-coated zinc-based coordination polymer composite prepared in Examples 1, 2, 3 and 4 of the present invention are shown.
[0036] Fig.10 The XRD diagrams of the hollow zinc silicate spheres prepared in Example 1 and the composites of hollow zinc silicate spheres coated with silicon dioxide prepared in Examples 2, 3 and 4 of the present invention are shown. DETAILED DESCRIPTION
[0037] The beneficial effects of the present invention are described in detail below in conjunction with the accompanying drawings and specific embodiments, which is intended to help readers better understand the essence of the present invention, but shall not constitute any limitation on the implementation and protection scope of the present invention.
[0038] Example 1
[0039] A method for preparing hollow ultramicrospheres with adjustable components and thickness:
[0040] Preparation of ZnCPs: Zinc nitrate hexahydrate, folic acid, and polyvinyl pyrrolidone were mixed and dissolved in a mixed solvent containing 24 mL of N,N-dimethylformamide and 8 mL of anhydrous ethanol, stirred at room temperature for 1 h, then transferred to a reactor, placed in an oven, and reacted at 100°C for 24 h. After the reaction was completed, the product was cooled to room temperature, collected by centrifugation, washed alternately with deionized water and anhydrous ethanol 3 times, and finally vacuum dried at 60°C for 24 h to obtain ZnCPs.
[0041] Preparation of ZnCPs@SiO2: Weigh 0.1g of zinc-based coordination polymer and 0.05g of hexadecyltrimethylammonium bromide, dissolve in a mixed solution of 3mL deionized water and 20mL anhydrous ethanol, stir ultrasonically until uniformly dispersed, stir for 20min, and control the water temperature of the ultrasound at 25℃, record as A solution; measure 400μL of ammonia water and add it to 20mL of anhydrous ethanol, record as B solution; add B solution to A solution under magnetic stirring, continue to stir evenly for 5min, then add 200μL of TEOS solution (tetraethyl orthosilicate), keep stirring at room temperature for 24h, collect by centrifugation after the reaction is completed, wash alternately with deionized water and anhydrous ethanol 3 times, and finally vacuum dry at 60℃ for 24h to obtain ZnCPs@SiO2. The dried sample is transferred to a crucible and calcined at 1000℃ in a muffle furnace for 4h, with a heating rate of 1℃ / min, to obtain the target product, hollow zinc silicate spheres.
[0042] like Figure 1 Shown is the SEM image of the prepared ZnCPs, which shows that its morphology is a uniformly dispersed spherical structure with an average particle size of about 400nm.
[0043] like Figure 2 Shown is the SEM image of ZnCPs@SiO2 in Example 1, whose morphology still maintains a regular spherical structure with an average particle size of about 440nm.
[0044] like Figure 3 The SEM image of Zn2SiO4 is shown. It can be seen from the figure that its particle size remains at about 440nm and the original spherical morphology is maintained.
[0045] like Figure 4 Shown is the TEM image of ZnCPs in Example 1. It can be seen from the image that the coordination polymer is a solid spherical structure with a smooth surface.
[0046] like Figure 5 The TEM image of ZnCPs@SiO2 in Example 1 is shown. It can be seen from the image that the coordination polymer is coated with a layer of silicon dioxide with a thickness of about 20 nm.
[0047] like Figure 6 The TEM image of Zn2SiO4 in Example 1 is shown. It can be seen from the image that it is a hollow spherical structure of uneven size, and there is no obvious silica shell layer on the surface.
[0048] Example 2
[0049] A method for preparing hollow ultramicrospheres with adjustable components and thickness, wherein the amount of TEOS added in Example 1 is changed to 400 μL:
[0050] Preparation of ZnCPs: Zinc nitrate hexahydrate, folic acid, and polyvinyl pyrrolidone were mixed and dissolved in a mixed solvent containing 24 mL of N,N-dimethylformamide and 8 mL of anhydrous ethanol, stirred at room temperature for 1 h, then transferred to a reactor, placed in an oven, and reacted at 100°C for 24 h. After the reaction was completed, the product was cooled to room temperature, collected by centrifugation, washed alternately with deionized water and anhydrous ethanol 4 times, and finally vacuum dried at 60°C for 24 h to obtain ZnCPs.
[0051] Preparation of ZnCPs@SiO2: Weigh 0.1g of zinc-based coordination polymer and 0.05g of hexadecyltrimethylammonium bromide, dissolve in a mixed solution of 3mL deionized water and 20mL anhydrous ethanol, stir ultrasonically until uniformly dispersed, stir for 25min, the water temperature of the ultrasound is controlled at 20℃, recorded as liquid A; measure 400μL of ammonia water and add it to 20mL of anhydrous ethanol, recorded as liquid B; add liquid B to liquid A under magnetic stirring, continue to stir evenly for 5min, then add 400μL of TEOS solution, keep stirring at room temperature for 24h, collect by centrifugation after the reaction is completed, wash alternately with deionized water and anhydrous ethanol for several times, and finally vacuum dry at 60℃ for 24h to obtain ZnCPs@SiO2. The dried sample is transferred to a crucible and calcined at 1000℃ in a muffle furnace for 4h with a heating rate of 1℃ / min to obtain the target product, silicon dioxide-coated zinc silicate hollow sphere composite material.
[0052] Example 3
[0053] A method for preparing hollow ultramicrospheres with adjustable components and thickness, wherein the amount of TEOS added in Example 1 is changed to 800 μL:
[0054] Preparation of ZnCPs: Zinc nitrate hexahydrate, folic acid, and polyvinyl pyrrolidone were mixed and dissolved in a mixed solvent containing 24 mL of N,N-dimethylformamide and 8 mL of anhydrous ethanol, stirred at room temperature for 1 h, then transferred to a reactor, placed in an oven, and reacted at 100°C for 24 h. After the reaction was completed, the product was cooled to room temperature, collected by centrifugation, washed alternately with deionized water and anhydrous ethanol 3 times, and finally vacuum dried at 60°C for 24 h to obtain ZnCPs.
[0055] Preparation of ZnCPs@SiO2: Weigh 0.1g of zinc-based coordination polymer and 0.05g of hexadecyltrimethylammonium bromide, dissolve in a mixed solution of 3mL deionized water and 20mL anhydrous ethanol, stir ultrasonically until uniformly dispersed, stir for 20min, and control the water temperature of the ultrasound at 30℃, which is recorded as liquid A; measure 400μL of ammonia water and add it to 20mL of anhydrous ethanol, which is recorded as liquid B; add liquid B to liquid A under magnetic stirring, continue to stir evenly for 5min, then add 800μL of TEOS solution, keep stirring at room temperature for 24h, collect by centrifugation after the reaction is completed, wash alternately with deionized water and anhydrous ethanol for several times, and finally vacuum dry at 60℃ for 24h to obtain ZnCPs@SiO2. The dried sample is transferred to a crucible and calcined at 1000℃ in a muffle furnace for 4h with a heating rate of 1℃ / min to obtain the target product, silicon dioxide-coated zinc silicate hollow sphere composite material.
[0056] Example 4
[0057] A method for preparing hollow ultramicrospheres with adjustable components and thickness, wherein the amount of TEOS added in Example 1 is changed to 1200 μL:
[0058] Preparation of ZnCPs: Zinc nitrate hexahydrate, folic acid, and polyvinyl pyrrolidone were mixed and dissolved in a mixed solvent containing 24 mL of N,N-dimethylformamide and 8 mL of anhydrous ethanol, stirred at room temperature for 1 h, then transferred to a reactor, placed in an oven, and reacted at 100°C for 24 h. After the reaction was completed, the product was cooled to room temperature, collected by centrifugation, washed alternately with deionized water and anhydrous ethanol 4 times, and finally vacuum dried at 60°C for 24 h to obtain ZnCPs.
[0059] Preparation of ZnCPs@SiO2: Weigh 0.1g of zinc-based coordination polymer and 0.05g of hexadecyltrimethylammonium bromide, dissolve in a mixed solution of 3mL deionized water and 20mL anhydrous ethanol, stir ultrasonically until uniformly dispersed, stir for 20min, and control the water temperature of the ultrasound at 40℃, record as A solution; measure 400μL of ammonia water and add it to 20mL of anhydrous ethanol, record as B solution; add B solution to A solution under magnetic stirring, continue to stir evenly for 5min, then add 1200μL of TEOS solution, keep stirring at room temperature for 24h, collect by centrifugation after the reaction is completed, wash alternately with deionized water and anhydrous ethanol for several times, and finally vacuum dry at 60℃ for 24h to obtain ZnCPs@SiO2. The dried sample is transferred to a crucible and calcined at 1000℃ in a muffle furnace for 4h with a heating rate of 1℃ / min to obtain the target product, silicon dioxide-coated zinc silicate hollow sphere composite material.
[0060] like Figure 7The SEM image of ZnCPs@SiO2 in Example 4 is shown, and its morphology still maintains a regular spherical structure with an average particle size of about 520 nm.
[0061] like Figure 8 The SEM image of Zn2SiO4@SiO2 in Example 4 is shown, and its morphology is a hollow spherical structure, and the average particle size is still about 520nm. There is an obvious silica shell layer on its surface with a thickness of about 60nm.
[0062] like Fig. 9 The XRD patterns of the composite materials of zinc-based coordination polymer coated with silicon dioxide formed by different TEOS addition amounts are shown. After adding TEOS, the diffraction peak of the zinc-based coordination polymer disappears due to the surface coating of silicon dioxide, and a broad peak of amorphous silicon dioxide is presented.
[0063] like Fig.10 The figure shows the XRD patterns of hollow zinc silicate spheres and hollow zinc silicate spheres composites coated with silicon dioxide prepared by calcining at 1000°C for 4h with different TEOS addition amounts. When TEOS = 200 μL, the calcined product is hollow zinc silicate spheres; when TEOS = 400 μL, the calcined product is hollow zinc silicate spheres composites coated with silicon dioxide (Zn2SiO4@SiO2), and a broad peak of amorphous SiO2 appears in the calcined product. As the amount of TEOS added continues to increase, the corresponding broad peak of SiO2 becomes more obvious, while the diffraction peak of zinc silicate becomes weaker. The amount of TEOS added can be adjusted according to the corresponding needs to obtain hollow zinc silicate spheres or hollow zinc silicate spheres composites coated with silicon dioxide of the desired thickness.
[0064] Both the zinc silicate hollow sphere and the silicon dioxide-coated zinc silicate hollow sphere composite have a large specific surface area, a unique reaction cavity, a good morphology and a novel structure. In addition, the silicon shell thickness of the silicon dioxide-coated zinc silicate hollow sphere composite is adjustable and has good biocompatibility.
[0065] The present invention provides a preparation idea and method for hollow zinc silicate spheres and hollow zinc silicate spheres with adjustable thickness. There are many methods and ways to implement the technical solution. The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the protection scope of the present invention. All components not specified in this embodiment can be implemented by existing technologies.
Claims
1. A method for preparing hollow ultramicrospheres with adjustable composition and thickness, characterized in that: The steps include: (1) dissolving zinc nitrate hexahydrate, folic acid, and polyvinyl pyrrolidone in a mixed solvent of N,N-dimethylformamide and anhydrous ethanol to obtain a mixed solution; (2) stirring the mixed solution uniformly, transferring the mixture into a reaction kettle, and placing the mixture into an oven for reaction to obtain a zinc-based coordination polymer; (3) washing the zinc-based coordination polymer with deionized water and anhydrous ethanol alternately and then vacuum drying to obtain ZnCPs; (4) ultrasonically dispersing the ZnCPs and hexadecyltrimethylammonium bromide in a mixed solution of deionized water and anhydrous ethanol, stirring them uniformly for the first time after ultrasonic dispersion, adding an ethanol solution containing ammonia water, stirring them uniformly for the second time, adding ethyl orthosilicate respectively, and then maintaining the mixture at room temperature for a third stirring reaction; (5) The obtained product was collected by centrifugation and washed alternately with deionized water and anhydrous ethanol, and then dried in a vacuum drying oven to obtain a zinc-based coordination polymer core-shell structure with different silica shell thicknesses. Finally, it was placed in a muffle furnace for calcination to obtain a zinc silicate with a hollow structure or a silica-coated zinc silicate hollow sphere composite with different shell thicknesses.
2. The preparation method according to claim 1, characterized in that In step (1), the amount of zinc nitrate hexahydrate is 0.5-3.0 mmol, folic acid is 0.05-0.5 g, polyvinyl pyrrolidone is 0.5-1.0 g, the molecular weight of polyvinyl pyrrolidone is 1300000, and the volumes of N,N-dimethylformamide and anhydrous ethanol are 24 mL and 8 mL, respectively.
3. The preparation method according to claim 1, characterized in that In step (2), the stirring time is 30 min to 60 min, and the reaction condition is 100° C. for 24 h.
4. The preparation method according to claim 1, characterized in that In step (3), the alternating washing is repeated three times, the drying temperature is 60° C., and the drying time is 24 h.
5. The preparation method according to claim 1, characterized in that In step (4), the amount of ZnCPs used is 0.1 g, hexadecyltrimethylammonium bromide is 0.05 g, deionized water is 3 mL, and anhydrous ethanol is 20 mL. The ultrasonic time is then 1 hour to make it evenly dispersed, and the first stirring is 20 minutes. The water temperature of the ultrasonication is controlled between 20 and 40 ° C.
6. The preparation method according to claim 1, characterized in that In step (4), the volumes of ammonia water and ethanol in the ammonia ethanol solution are 400 μL and 20 mL, respectively, the second stirring time is 5 min, the amount of ethyl orthosilicate is 200 μL to 1200 μL, and the third stirring time is 24 h.
7. The preparation method according to claim 1, characterized in that In step (5), the drying temperature is 60° C. and the drying time is 24 h.
8. The preparation method according to claim 1, characterized in that In step (5), the calcination temperature is 1000° C., the calcination time is 4 h, and the heating rate is 1° C. / min.
9. The hollow ultramicrospheres with adjustable composition and thickness obtained by the method according to any one of claims 1 to 8, characterized in that: The hollow ultramicrospheres have a large specific surface area and a reaction cavity. The hollow ultramicrospheres are specifically zinc silicate or silicon dioxide-coated zinc silicate hollow sphere composites with a hollow structure. The thickness of silicon dioxide in the silicon dioxide-coated zinc silicate hollow sphere composite can be adjusted.
10. The use of hollow ultramicrospheres with adjustable composition and thickness according to claim 9, characterized in that: The hollow ultramicrospheres can be used to adsorb heavy metal ions and organic pollutants in industrial wastewater, and to catalyze the reduction of gaseous pollutants such as NO, CO, and CO. They can also be used in energy storage, chemical reactors, biomedicine, drug delivery, sensing, optoelectronic devices, information encryption, drug loading, and bioimaging.
Citation Information
Patent Citations
Preparation method of zinc silicate hollow micron ball
CN105502421A
Preparation method of green long-afterglow luminescent material
CN114369457A