Easy-to-clean mining low-temperature leaking stoppage waterproof inorganic spraying material and application thereof
By using inorganic spray materials composed of cement, heat-reducing cement and nanomaterials, the problems of high-temperature fire and construction brittleness of spraying and plugging materials during the reaction process are solved, low-temperature curing, flexibility and easy cleaning are achieved, and coal mines are improved Well safety and construction efficiency.
Patent Information
- Application Number
- CN202411248511.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-26
AI Technical Summary
The existing spraying and leak-blocking materials generate high temperatures during the reaction process, pose a fire risk, and are highly brittle during the construction process and are prone to block the nozzles and pipelines, which increases the construction difficulty and maintenance costs, and fails to provide a safe and cost-effective solution.
Using inorganic spraying materials consisting of cement, heat-reducing cement, nanomaterials, modified chopped fibers, continuous fibers, bio-based plasticizers and high-efficiency rheology modifiers, low-temperature curing is achieved by controlling the reaction temperature and addition ratio. , improve flexibility and easy cleaning, and use environmentally friendly non-toxic materials.
It effectively reduces fire risk, improves the flexibility and sealing effect of materials, simplifies the cleaning process, reduces maintenance costs, and ensures the safety and efficiency of construction.
Smart Images

Figure CN119019140A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of spraying materials, and in particular to an easy-to-clean low-temperature leak-proof and waterproof inorganic spraying material for mining and application thereof. Background Art
[0002] Spray plugging technology has always been a popular method for preventing air leaks and waterproofing underground in coal mines. Polyurethane foam and cement-based materials are traditional choices, each with its own advantages and disadvantages. Polyurethane foam is widely used in emergency plugging and structural reinforcement due to its excellent sealing and rapid response properties, but its high cost and high heat release during application have always been technical bottlenecks. On the other hand, cement-based inorganic materials are widely used due to their low cost and good durability, but the problems they face in pipeline transportation and construction are equally prominent. Driven by technological advances, the R&D team continues to explore safer and more economical spraying materials, striving to achieve the dual effects of efficient plugging and waterproofing.
[0003] Although the existing technology provides a basic solution, there are still many shortcomings in practical applications, which seriously limit the possibility of its widespread application. First, the high temperature generated by traditional polyurethane foam materials during the reaction process may trigger underground fires, which is particularly dangerous in mine environments with extremely high safety requirements. Secondly, although cement-based materials have cost advantages, they are brittle and easy to clog nozzles and pipes during transportation and construction, which increases the difficulty of construction and maintenance costs. Although the low-heat polyurethane filling material proposed in CN105175673A reduces the reaction temperature to 82.5°C to 85°C, this temperature is still relatively high and fails to effectively avoid the risk of fire. At the same time, there is still the problem of clogging equipment. Therefore, the existing technology has failed to provide a comprehensive solution that is both safe and cost-effective. In particular, there is still a lot of room for improvement in ensuring construction safety and simplicity.
[0004] The core goal of the present invention is to develop an inorganic spray material that can quickly form a sealed structure without generating high temperatures, effectively reducing the risk of fire. In addition, the material of the present invention needs to be highly flexible to adapt to complex underground environments, while ensuring that the material will not crack due to shrinkage or the passage of time after construction. Importantly, this new material has a controllable setting time and high early strength, ensuring rapid curing and load-bearing capacity after construction. Most importantly, the new material should be easy to clean, and even after a long period of spraying, the equipment can be cleaned with clean water, which greatly simplifies maintenance work and reduces overall operating costs. By solving these technical problems, the new material will greatly improve coal mine safety and construction efficiency, filling the gaps in existing technologies. Summary of the Invention
[0005] In order to achieve the above-mentioned purpose of the invention and to solve the above-mentioned technical problems, the present invention provides an easy-to-clean low-temperature leak-proof and waterproof inorganic spraying material for mining, characterized in that the spraying material is made of the following raw materials in parts by mass:
[0006] 30-40 parts of cement, 5-10 parts of heat-reducing cement, 45-55 parts of quartz sand, 1-3 parts of nanomaterials, 1-4 parts of ultrafine nanomaterials, 0.3-1 parts of thickener, 0.2-1 parts of high-efficiency rheology modifier, 0.5-1 parts of modified chopped fibers, 0.5-1.5 parts of continuous fibers, 0.2-0.5 parts of hydrophobic agent, 5-10 parts of adhesive, 0.3-1 parts of bio-based plasticizer, and 0.4-1 parts of retarder.
[0007] Preferably, the cement is silicate cement with a grade of PO≥42.5.
[0008] Preferably, the quartz sand is 100-200 mesh continuously graded natural river sand or 70-140 mesh quartz sand.
[0009] Preferably, the nano material is nano silicon with a particle size of 30-50 nm, and the ultrafine nano material is ultrafine nano calcium with a particle size of 10-30 nm.
[0010] Preferably, the high-efficiency rheology modifier is organic expansive soil.
[0011] Preferably, the chopped fibers are polypropylene fibers and bamboo fibers with a mass ratio of 7:3-7:1 and a length of 10-20 mm; the continuous fibers are glass fibers with a length of 10-15 μm.
[0012] Preferably, the bio-based plasticizer is epoxidized soybean oil or polylactic acid.
[0013] Preferably, the retarder is a hydroxycarboxylate.
[0014] The present invention also provides a method for preparing the easy-to-clean low-temperature leak-proof and waterproof inorganic spraying material for mining:
[0015] S1 immerses the chopped fibers in methyltrimethoxysilane solution, covers them evenly, and solidifies them at 80°C to form modified chopped fibers; S2 puts cement, heat-reducing cement, quartz sand, adhesive, nanomaterials, and modified chopped fibers into a stirring kettle, controls the speed to 50 rpm, controls the temperature to 20-30°C, stirs for 20 minutes, and allows to stand for 5 minutes.
[0016] S3 adds thickener, continuous fiber, ultrafine nanomaterial, and retarder, controls the speed to 60 rpm, the temperature to 20-30°C, and stirs for 15 minutes;
[0017] S4 added hydrophobic agent, bio-based plasticizer, and high-efficiency rheology modifier and continued stirring for 15 minutes. After stirring, sampling was performed.
[0018] The present invention also provides an application of an easy-to-clean low-temperature leak-plugging and waterproof inorganic spray material for mining. The above-mentioned spray material is adjusted to a water-cement ratio of 0.2-0.4, and then added to a spraying equipment for spraying. After spraying is completed, clean water is used to clean the high-efficiency mixing system and the spray pipe and nozzle in the spraying equipment.
[0019] The beneficial effects brought about by the technical solution provided by the present invention are:
[0020] Low Reaction Temperature: By utilizing cement, heat-reducing cement, and specialized nanomaterials, the spray material of this invention significantly reduces the heat generated during the curing process, effectively preventing fire hazards caused by excessively high reaction temperatures in enclosed environments such as mines. This directly addresses the potential safety hazards associated with high reaction temperatures in existing technologies.
[0021] High flexibility and crack resistance: The combination of chopped and continuous fibers not only enhances the material's mechanical strength but also provides high flexibility, making it less prone to cracking after hardening, thereby ensuring long-term sealing and structural integrity. This effectively addresses the cracking and sealing failure issues that can occur with traditional materials over long periods of use.
[0022] Easy to clean: By incorporating bio-based plasticizers and high-efficiency rheology modifiers, the material allows spray equipment to be easily cleaned with water after application, significantly simplifying cleaning and reducing maintenance costs. This is crucial for addressing the issue of existing spray nozzles and pipes being prone to clogging and difficult to clean.
[0023] Environmentally friendly: All raw materials are environmentally friendly and non-toxic, ensuring that the materials are harmless to the environment and operators during use. Compared with traditional spray materials containing harmful substances, the materials of this invention are safer and help improve the working environment.
[0024] Controllable setting time and high early strength: By precisely controlling the addition ratio of the retarder and the application of ultrafine nanomaterials, the curing speed of the material of the present invention can be adjusted according to site needs, while ensuring that high strength is achieved early, supporting rapid continuation of construction activities. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 These are sample photos of Example 1(a), Example 4(b), Example 8(c), and Example 9(d) of the present invention.
[0026] Figure 2 This is a photo of the waterproof experiment of Example 1 of the present invention.
[0027] Figure 3 This is a photo of the indoor spraying experiment of Example 1 of the present invention.
[0028] Figure 4 This is a photo of the outdoor spraying experiment of Example 1 of the present invention.
[0029] Figure 5 This is a photo of the spraying application of the mine protection net according to Example 1 of the present invention.
[0030] Figure 6 This is a photo of the mine leak plugging method according to Example 1 of the present invention.
[0031] Figure 7 This is a photo of the mine leak plugging method according to Example 1 of the present invention. DETAILED DESCRIPTION
[0032] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention will be further described in detail below in conjunction with the embodiments. Of course, the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0033] Example 1
[0034] An easy-to-clean low-temperature leak-proof and waterproof inorganic spraying material for mining:
[0035] S1 completely immersed polypropylene fiber and bamboo fiber with a length of 15 mm and a mass ratio of 7:2 in methyltrimethoxysilane
[0036] In solution, it is cured at 80°C to form modified chopped fibers;
[0037] S2: 35 parts of Portland cement (label PO 425), 6 parts of heat-reducing cement, 50 parts of 100-200 mesh continuous graded natural river sand, 5 parts of adhesive (dispersible latex powder N), 2 parts of nano-silicon with a particle size of 50nm and 0.8 parts of modified short-cut fibers were put into a stirring tank, the speed was controlled at 50 rpm, the temperature was controlled at 30°C, stirred for 20 minutes, and allowed to stand for 5 minutes;
[0038] S3 added 0.5 parts of thickener (starch ether), 1.2 parts of glass fiber with a length of 15 μm, 3 parts of ultrafine nano calcium with a particle size of 20 nm, and 0.5 parts of naphthalene retarder (FDN-C water reducer), controlled the speed to 60 rpm, the temperature to 20-30°C, and stirred for 15 minutes;
[0039] S4 add 0.3 parts of water repellent (WACKER Powder A), 0.6 parts of epoxidized soybean oil, and 0.25 parts of organic expansive soil were stirred for 15 minutes, and samples were taken after stirring was completed.
[0040] The water-cement ratio during use is 0.3, and it is added to the spraying equipment for spraying. After the spraying is completed, use clean water to clean the high-efficiency mixing system, spray pipes and nozzles in the spraying equipment.
[0041] Example 2
[0042] The method is the same as that in Example 1, except that the quartz sand is 70-140 mesh quartz sand.
[0043] Example 3
[0044] The same preparation method as in Example 1 was used, except that 1 part of nano-silicon was used.
[0045] Example 4
[0046] The same preparation method as in Example 1 was used, except that 3 parts of nano-silicon were used.
[0047] Example 5
[0048] The same preparation method as in Example 1 was used, except that 0.5 parts of modified short-cut fibers were used.
[0049] Example 6
[0050] The same preparation method as in Example 1 was used, except that 1 part of modified short-cut fiber was used.
[0051] Example 7
[0052] The same preparation method as in Example 1 was used, except that 0.5 parts of glass fiber was used.
[0053] Example 8
[0054] The same preparation method as in Example 1 was used, except that 1.5 parts of modified short-cut fibers were used.
[0055] Example 9
[0056] The same preparation method as in Example 1 was used, except that 0.3 parts of epoxidized soybean oil was used.
[0057] Example 10
[0058] The same preparation method as in Example 1 was used, except that 1 part of epoxidized soybean oil was used.
[0059] Example 11
[0060] The same preparation method as in Example 1 was used, except that the water-cement ratio was 0.2.
[0061] Example 12
[0062] The same preparation method as in Example 1 was used, except that the water-cement ratio was 0.4.
[0063] Example 13
[0064] The preparation method is the same as that of Example 1, except that 1 part of ultrafine nano calcium is added.
[0065] Example 14
[0066] The same preparation method as in Example 1 was used, except that 4 parts of ultrafine nano-calcium were added.
[0067] Example 15
[0068] An easy-to-clean low-temperature leak-proof and waterproof inorganic spraying material for mining:
[0069] S1: Polypropylene fiber and bamboo fiber with a length of 10 mm and a mass ratio of 7:3 are completely immersed in methyltrimethoxysilane solution and cured at 80°C to form modified short fibers;
[0070] S2 30 parts of Portland cement (label PO425), 10 parts of heat-reducing cement, 45 parts of 100-200 mesh continuous graded natural river sand, 10 parts of adhesive (dispersible latex powder N), 2 parts of nano-silicon with a particle size of 30nm and 0.8 parts of modified short-cut fibers were put into a stirring tank, the speed was controlled at 50 rpm, the temperature was controlled at 20°C, stirred for 20 minutes, and allowed to stand for 5 minutes.
[0071] S3 added 0.3 parts of thickener (starch ether), 1.2 parts of glass fiber with a length of 10-15 microns, 3 parts of ultrafine nano calcium with a particle size of 30 nm, and 0.4 parts of naphthalene retarder (FDN-C water reducer), controlled the speed to 60 rpm, the temperature to 20°C, and stirred for 15 minutes;
[0072] S4 add 0.5 parts of water repellent (WACKER Powder A), 0.6 parts of epoxidized soybean oil, and 0.2 parts of organic expansive soil were stirred for 15 minutes, and samples were taken after stirring was completed.
[0073] The water-cement ratio during use is 0.3, and it is added to the spraying equipment for spraying. After the spraying is completed, use clean water to clean the high-efficiency mixing system, spray pipes and nozzles in the spraying equipment.
[0074] Example 16
[0075] An easy-to-clean low-temperature leak-proof and waterproof inorganic spraying material for mining:
[0076] S1: Polypropylene fiber and bamboo fiber with a length of 20 mm and a mass ratio of 7:1 are completely immersed in a methyltrimethoxysilane solution and cured at 80°C to form modified short fibers;
[0077] S2: 40 parts of Portland cement (label PO425), 5 parts of heat-reducing cement, 55 parts of 100-200 mesh continuous graded natural river sand, 5 parts of adhesive (dispersible latex powder N), 2 parts of nano-silicon with a particle size of 50nm and 0.8 parts of modified short-cut fibers were put into a stirring tank, the speed was controlled at 50 rpm, the temperature was controlled at 30°C, stirred for 20 minutes, and allowed to stand for 5 minutes.
[0078] S3: Add 1 part of thickener (starch ether), 1.2 parts of glass fiber with a length of 10-15 microns, 3 parts of ultrafine nano calcium with a particle size of 10 nm, and 1 part of naphthalene retarder (FDN-C water reducer), control the speed to 60 rpm, the temperature to 30°C, and stir for 15 minutes;
[0079] S4 add 0.2 parts of water repellent (WACKER Powder A), 0.6 parts of epoxidized soybean oil, and 1 part of organic expansive soil, and continue stirring for 15 minutes. After stirring, take samples.
[0080] The water-cement ratio during use is 0.3, and it is added to the spraying equipment for spraying. After the spraying is completed, use clean water to clean the high-efficiency mixing system, spray pipes and nozzles in the spraying equipment.
[0081] Comparative Example 1
[0082] The preparation was carried out according to the same preparation method as in Example 1, except that the polypropylene fiber and bamboo fiber were used directly without any modification process.
[0083] Comparative Example 2
[0084] The preparation method is the same as that in Example 1, except that no nano-silicon material is added.
[0085] Comparative Example 3
[0086] The preparation was carried out in the same manner as in Example 1, except that no modified short fibers were added.
[0087] Comparative Example 4
[0088] The same preparation method as in Example 1 was used, except that no glass fiber was added.
[0089] Comparative Example 5
[0090] The same preparation method as in Example 1 was used, except that DOP plasticizer was used.
[0091] Comparative Example 6
[0092] The same preparation method as that of Comparative Example 1 was used, except that the polypropylene fiber and bamboo fiber were replaced by PP fiber.
[0093] Comparative Example 7
[0094] The preparation method is the same as that of Example 1, except that the chopped fibers are replaced with glass fibers.
[0095] Comparative Example 8
[0096] The same preparation method as in Example 1 was used for the preparation, except that the short fibers and glass fibers were replaced by PP fibers.
[0097] Comparative Example 9
[0098] The preparation method is the same as that of Example 1, except that ultrafine nano-calcium is not added.
[0099] Comparative Example 10
[0100] Inorganic spraying materials are sold on the market (inorganic spraying materials produced by Beijing Ruinuo Company).
[0101] Experimental test:
[0102] 1. Surface drying time: according to standard GB1728-2020;
[0103] 2. Flexural strength and compressive strength: GB / T 17671-2021;
[0104] 3. Tensile strength, bond strength, elongation at break: GB / T16777-2008
[0105] 4. Reaction temperature: AQ / T 1089-2020
[0106] 5. Waterproofness: GB 23440-2009
[0107] 6. Film forming time: Q / 0800BHMC-017—2024
[0108] Table 1 Experimental test data
[0109]
[0110]
[0111] Example 1 performs best: According to the test results, Example 1 performs best in all performance indicators, especially in flexural strength, compressive strength, tensile strength, and elongation at break. This shows that the combined use of modified chopped fibers, carefully selected nano-silicon, and ultrafine nano-calcium, along with optimized ratios and processing, can significantly improve the material's structural and mechanical properties.
[0112] Comparative Example 10 performed the worst: Comparative Example 10, a conventional inorganic spraying material on the market, had significantly lower performance than the examples in all indicators, especially in terms of flexural strength and compressive strength. This emphasizes the importance of the technical improvements and optimized formulations of the present invention.
[0113] Effects of modified chopped fibers and nanomaterials: All examples containing these components exhibited improved mechanical properties and lower reaction temperatures compared to formulations without modified fibers (Comparative Example 3) or nanomaterials (Comparative Example 2). This demonstrates the critical role of these materials in improving overall performance and safety.
[0114] Ease of cleaning: All examples performed well in film-forming time and tack-free time, with Example 1 in particular performing the best in these tests, supporting the material's easy-to-clean nature. This improved cleaning efficiency not only reduces maintenance costs but also improves operational efficiency.
[0115] Environmental protection and safety performance: The test results of reaction temperature show that the reaction temperature of the material of the present invention is generally low (28-30°C on average), which helps to reduce safety risks when used in closed or low-ventilation environments, such as mines.
[0116] Structural integrity and long-term performance: High flexural and compressive strengths, as well as high elongation at break, indicate that the material of the present invention has excellent structural integrity and crack resistance, which is critical for ensuring long-term sealing effect and structural integrity.
[0117] In summary
[0118] By incorporating modified chopped fibers, carefully selected nanomaterials, and optimized processes, the material system of this invention successfully achieves the technical goals of high strength, low reaction temperature, easy cleaning, and high environmental safety, significantly outperforming existing products on the market. These improvements not only enhance the product's performance but also increase its application value in low-temperature leak plugging and waterproofing applications in mines.
[0119] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. An easy-to-clean low-temperature leak-proof and waterproof inorganic spraying material for mining, characterized in that: The spraying material is made of the following raw materials in parts by mass: 30-40 parts of cement, 5-10 parts of heat-reducing cement, 45-55 parts of quartz sand, 1-3 parts of nanomaterials, 1-4 parts of ultrafine nanomaterials, 0.3-1 parts of thickener, 0.2-1 parts of high-efficiency rheology modifier, 0.5-1 parts of modified chopped fibers, 0.5-1 parts of continuous fibers, 0.2-0.5 parts of hydrophobic agent, 5-10 parts of adhesive, 0.3-1 parts of bio-based plasticizer, and 0.4-1 parts of retarder.
2. The spraying material according to claim 1, characterized in that: The cement is silicate cement with a grade of PO≥42.
5.
3. The spraying material according to claim 1, characterized in that: The quartz sand is 100-200 mesh continuous graded natural river sand or 70-140 mesh quartz sand.
4. The spraying material according to claim 1, characterized in that: The nano material is nano silicon with a particle size of 30-50nm, and the ultrafine nano material is ultrafine nano calcium with a particle size of 10-30nm.
5. The spraying material according to claim 1, characterized in that: The high-efficiency rheology modifier is organic expansive soil.
6. The spraying material according to claim 1, characterized in that: The chopped fibers are polypropylene fibers and bamboo fibers, with a mass ratio of 7:3-7:1 and a length of 10-20 mm; the continuous fibers are glass fibers, with a length of 10-15 μm.
7. The spraying material according to claim 1, characterized in that: The bio-based plasticizer is epoxidized soybean oil or polylactic acid.
8. The spraying material according to claim 1, characterized in that: The retarder is a hydroxycarboxylate.
9. A method for preparing an easy-to-clean low-temperature leak-proof and waterproof inorganic spray material for mining according to any one of claims 1 to 8: S1 immerses the chopped fibers in a methyltrimethoxysilane solution, covers them evenly, and cures them at 80°C to form modified chopped fibers; S2 puts cement, heat-reducing cement, quartz sand, adhesive, nanomaterials and modified chopped fibers into a stirring tank. Control the speed to 50 rpm, the temperature to 20-30°C, stir for 20 minutes, let stand for 5 minutes, S3 adds thickener, continuous fiber, ultrafine nanomaterial, and retarder, controls the speed to 60 rpm, the temperature to 20-30°C, and stirs for 15 minutes; S4 added hydrophobic agent, bio-based plasticizer and high-efficiency rheology modifier and continued stirring for 15 minutes. After stirring, sampling was performed.
10. An application of an easy-to-clean low-temperature leak-proof and waterproof inorganic spraying material for mining, characterized in that: The spray material of any one of claims 1 is adjusted to a water-cement ratio of 0.2-0.4, and then added to a spraying device for spraying. After the spraying is completed, the high-efficiency mixing system, the spray pipe and the nozzle in the spraying device are cleaned with clean water.