Ceramic silicone rubber material and preparation method thereof
By using a combination of porcelain filler and methylvinyl silicone rubber in ceramicized silicone rubber materials, molding at room temperature and porcelain strength below 500°C are achieved, and the poor porcelain-forming effect of existing ceramicized silicone rubber materials is solved. The problem of this problem improves the temperature resistance and reduces production costs.
Patent Information
- Application Number
- CN202411101096.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-12
AI Technical Summary
The existing ceramic silicone rubber materials have poor porcelain formation effects in high temperature environments, requiring professional equipment and high temperature molding, with high cost, and low bending strength, high shrinkage rate, and poor temperature resistance when below 800℃.
The ceramicized silicone rubber material consisting of methyl vinyl silicone rubber and porcelain filler is used. The porcelain filler consists of the filler body, a solvent, a bonding aid, a thermal compensation agent, a shrinkage inhibitor and a flame retardant, and passes through room temperature. The process of under-vulcanization and heating ceramicization achieves a ceramicization strength below 500°C, and improves the temperature resistance and mechanical properties through eutectic reaction.
The ceramic silicone rubber is formed at room temperature, with high ceramic strength, low shrinkage and high bending strength at 500°C, and excellent temperature resistance, reducing production and manufacturing costs.
Smart Images

Figure CN119019180A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of silicone rubber, and in particular to a ceramic silicone rubber material and a preparation method thereof. Background Art
[0002] Ceramic silicone rubber materials are similar to ordinary rubber materials at room temperature, and are non-toxic, high temperature resistant, have excellent electrical insulation properties, and good processing properties. When placed in a high temperature environment, the material can be transformed from a flexible rubber to a hard ceramic body, ensuring the safety of the material. Especially in the fields of aerospace, sealing, power transmission, construction, and electronics and electrical, ceramic silicone rubber that is fire-resistant and flame-retardant and has a certain strength has become a new demand point.
[0003] However, while the research field of ceramic silicone rubber has become more and more multi-faceted and multi-level, it still faces many challenges: on the one hand, in the preparation process of ceramic silicone rubber composite materials, in order to realize the ceramic function of silicone rubber, silicone rubber is usually mixed with a large amount of ceramic filler in an open mixer or an internal mixer, and then vulcanized and formed at high temperature by professional equipment; however, this method requires the use of professional equipment and needs to be formed at high temperature, which makes the production and manufacturing costs too high; on the other hand, the existing ceramic silicone rubber usually needs to undergo a eutectic reaction at a temperature above 800°C to obtain a higher strength. When it is below 800°C, the ceramic effect is poor, and the bending strength is only about 2-3MPa; in addition, due to the addition of a large amount of co-solvents, although the ceramic transition temperature is lowered, the shrinkage rate of silicone rubber in the ceramic process is higher, and the temperature resistance is poor.
[0004] Therefore, based on the above problems, there is an urgent need to provide a new ceramic silicone rubber material and a preparation method thereof. Summary of the invention
[0005] The embodiment of the present invention provides a ceramic silicone rubber material and a preparation method thereof. The ceramic silicone rubber can be molded at room temperature and has porcelain strength at 500°C. The ceramic silicone rubber formed after porcelainization has a low shrinkage rate, high bending strength and temperature resistance.
[0006] In a first aspect, the present invention provides a ceramic silicone rubber material, which is composed of silicone rubber and a ceramic filler; wherein the ceramic filler is composed of a filler body, a solvent, a bonding aid, a thermal compensator, a shrinkage inhibitor and a flame retardant.
[0007] Preferably, the methyl vinyl silicone rubber contains a platinum catalyst, and the content of the platinum catalyst is 0.5-1.0% of the total amount of the methyl vinyl silicone rubber;
[0008] The viscosity of the methyl vinyl silicone rubber is 5000-20000 mPa·s, and the mass ratio of the methyl vinyl silicone rubber to the ceramic filler is 100:(100-200).
[0009] Preferably, the filler body is alumina, and the flux is low-melting-point glass powder.
[0010] Preferably, the bonding aid is at least one of aluminum dihydrogen phosphate, aluminum polyphosphate or aluminum metaphosphate.
[0011] Preferably, the thermal compensator is composed of silicon powder and aluminum powder; wherein the mass ratio of silicon powder to aluminum powder is (5-20): (5-20).
[0012] Preferably, the shrinkage inhibitor is alumina fiber cotton; wherein the fiber diameter of the alumina fiber cotton is 3-4 microns.
[0013] Preferably, the flame retardant is aluminum hydroxide.
[0014] Preferably, the composition of the ceramic filler is as follows, measured in parts by weight: 40-80 parts of filler body, 10-20 parts of cosolvent, 0.5-5 parts of bonding aid, 10-40 parts of thermal compensator, 0.5-5 parts of shrinkage inhibitor and 5-13 parts of flame retardant.
[0015] More preferably, the composition of the ceramic filler is as follows: 55-65 parts of filler body, 15-18 parts of solvent, 2-3 parts of bonding aid, 15-25 parts of thermal compensator, 2-3 parts of shrinkage inhibitor and 12-13 parts of flame retardant.
[0016] In a second aspect, the present invention provides a method for preparing the ceramic silicone rubber material according to any one of the first aspects above, the preparation method comprising the following steps:
[0017] (1) stirring and mixing the methyl vinyl silicone rubber and the porcelain-forming filler to obtain a mixed material;
[0018] (2) placing the mixed material in a mold for vulcanization reaction to obtain a flexible silicone rubber;
[0019] (3) placing the flexible silicone rubber in a muffle furnace for heating and ceramicization to obtain the ceramic silicone rubber.
[0020] Preferably, in step (2), the temperature of the sulfurization reaction is 22-24° C., and the time is 7-10 days.
[0021] Preferably, the temperature of the vulcanization reaction is 40-42° C. and the time is 5-6 hours.
[0022] Preferably, in step (3), the temperature of the heating ceramicization is 500-1600°C, the heating rate is 10-30°C / min, and the time is 30-90min.
[0023] Compared with the prior art, the present invention has at least the following beneficial effects:
[0024] The ceramic silicone rubber material of the present invention is composed of methyl vinyl silicone rubber and a ceramic filler. After the methyl vinyl silicone rubber and the ceramic filler are mixed, they can be formed at room temperature without the need for professional equipment and secondary vulcanization. In addition, the ceramic filler composed of a filler body, a cosolvent, a bonding aid, a thermal compensator, a shrinkage inhibitor and a flame retardant has good ceramic strength at 500°C. During the ceramic forming process, the methyl vinyl silicone rubber will undergo thermal decomposition, and by optimizing the components in the ceramic filler, the methyl vinyl silicone rubber after thermal decomposition will undergo a eutectic reaction with the components in the ceramic filler, so that the formed ceramic silicone rubber has both excellent temperature resistance and mechanical properties, as well as a lower shrinkage rate. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0026] Figure 1 1 is an XRD diagram of a ceramic silicone rubber material provided in Example 1 of the present invention at different temperatures; wherein the abscissa is the incident angle of the x-ray, and the ordinate is the diffraction intensity;
[0027] Figure 2 This is a diagram showing the macroscopic appearance changes of a ceramicized silicone rubber material provided in Example 1 of the present invention after being ceramicized at 1600° C. for different periods of time;
[0028] Figure 3 This is a diagram showing the macroscopic appearance changes of a ceramicized silicone rubber material provided in Example 1 of the present invention after being ceramicized at different temperatures; in the diagram, the temperatures from top to bottom are 500° C., 600° C., 800° C., 1000° C., 1200° C., 1400° C. and 1600° C.;
[0029] Figure 4 This is a diagram showing the macroscopic appearance changes of a ceramicized silicone rubber material provided in Example 2 of the present invention after being ceramicized at different temperatures;
[0030] Figure 5 This is a diagram showing the macroscopic appearance changes of a ceramicized silicone rubber material provided in Example 3 of the present invention after being ceramicized at different temperatures;
[0031] Figure 6 This is a diagram showing the macroscopic appearance changes of a ceramicized silicone rubber material provided in Example 4 of the present invention after being ceramicized at different temperatures;
[0032] Figure 7 This is a diagram showing the macroscopic appearance changes of a ceramicized silicone rubber material provided in Example 5 of the present invention after being ceramicized at different temperatures;
[0033] Figure 8 This is a diagram showing the macroscopic appearance changes of a ceramicized silicone rubber material provided in Example 6 of the present invention after being ceramicized at different heating rates to 1600° C.;
[0034] Fig. 9 This is a diagram showing the macroscopic appearance changes of a ceramicized silicone rubber material before and after ceramicization provided in Comparative Example 4 of the present invention. DETAILED DESCRIPTION
[0035] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0036] The invention provides a ceramic silicone rubber material, which consists of methyl vinyl silicone rubber and a ceramic filler; wherein the ceramic filler consists of a filler body, a cosolvent, a bonding aid, a thermal compensator, a shrinkage inhibitor and a flame retardant.
[0037] The ceramic silicone rubber material in the embodiment of the present invention is composed of methyl vinyl silicone rubber and a ceramic filler. After the methyl vinyl silicone rubber and the ceramic filler are mixed, they can be formed at room temperature without the need for professional equipment and secondary vulcanization; and the ceramic filler composed of a filler body, a cosolvent, a bonding aid, a thermal compensator, a shrinkage inhibitor and a flame retardant has good ceramic strength at 500°C. During the ceramic forming process, the methyl vinyl silicone rubber will undergo thermal decomposition. By optimizing the components in the ceramic filler, the methyl vinyl silicone rubber after thermal decomposition undergoes a eutectic reaction with the components in the ceramic filler, so that the formed ceramic silicone rubber has excellent temperature resistance and mechanical properties, as well as a lower shrinkage rate.
[0038] According to some preferred embodiments, the methyl vinyl silicone rubber contains a platinum catalyst, and the content of the platinum catalyst is 0.5-1.0% of the total amount of the methyl vinyl silicone rubber (for example, it can be 0.5%, 0.8%, 0.9% or 1.0%); the viscosity of the methyl vinyl silicone rubber is 5000-20000 mPa·s (for example, it can be 5000 mPa·s, 8000 mPa·s, 10000 mPa·s, 15000 mPa·s or 20000 mPa·s), and the mass ratio of the methyl vinyl silicone rubber to the porcelain filler is 100:(100-200) (for example, it can be 100:100, 100:150 or 100:200).
[0039] In the embodiment of the present invention, methyl vinyl silicone rubber of a certain viscosity is selected and supplemented with a certain amount of ceramic filler. The two can be vulcanized and formed at room temperature. The molding process is simple and does not require professional equipment and secondary vulcanization reaction. In addition, by controlling the mass ratio of methyl vinyl silicone rubber to ceramic filler, it is beneficial to prepare a ceramic silicone rubber material with excellent high temperature resistance, mechanical properties and low thermal shrinkage performance. It has been confirmed by the experiment of the present invention that with the increase of the amount of ceramic filler added, it is beneficial to ensure a lower mass loss rate and a lower shrinkage rate of the ceramic silicone rubber material, and at the same time it is beneficial to enhance the mechanical strength of the ceramic silicone rubber material. However, the amount of ceramic filler added should not be too much. When the ceramic filler is too much, the viscosity will be too large, which will easily cause the ceramic filler to agglomerate and the mixing uniformity of the ceramic filler cannot be guaranteed, thereby affecting the ceramic performance. At the same time, the viscosity is high and the process performance is greatly reduced.
[0040] According to some preferred embodiments, the filler body is alumina, the flux is low-melting-point glass powder; and the bonding aid is at least one of aluminum dihydrogen phosphate, aluminum polyphosphate or aluminum metaphosphate.
[0041] In the embodiment of the present invention, alumina is used as the filler body of the ceramic filler. On the one hand, alumina is a very good silicone rubber reinforcing filler. On the other hand, alumina has good temperature resistance, has a stable crystal phase at high temperature, and can react with other components in the ceramic filler, thereby further ensuring that the ceramic silicone rubber material has excellent temperature resistance; low-melting point glass powder with a melting point of 350-580°C is used as a solvent. The low-melting point glass powder can melt at a temperature below 600 degrees. While filling the gap, it is beneficial to the eutectic reaction of the ceramic filler, thereby improving the mechanical properties of the ceramic silicone rubber; at the same time, aluminum dihydrogen phosphate, aluminum polyphosphate and / or aluminum metaphosphate are used as bonding aids. Before the eutectic reaction occurs, the above-mentioned types of raw materials can exert bonding characteristics, enhance the mechanical strength of the ceramic silicone rubber material, and transform into Al(PO)4 at high temperature, which can still play a good bonding role, thereby further enhancing the mechanical strength of the ceramic silicone rubber in a high temperature environment.
[0042] According to some preferred embodiments, the thermal compensator is composed of silicon powder and aluminum powder; wherein the mass ratio of silicon powder to aluminum powder is (5-20):(5-20) (for example, it can be 5:5, 5:15, 5:20, 5:10, 10:5, 20:5, 15:5, 15:20 or 20:20).
[0043] In the embodiment of the present invention, silicon powder and aluminum powder are used as thermal compensators during the ceramicization process. On the one hand, silicon powder and aluminum powder can undergo oxidation reaction at a certain temperature and in a certain oxygen environment to form silicon dioxide and aluminum oxide with certain temperature resistance, thereby producing thermal compensation, reducing the mass loss rate, and compensating for shrinkage; on the other hand, when a higher ceramicization temperature is reached, the products formed by the oxidation of silicon powder and aluminum powder can further react with other components to form a high-temperature resistant ceramic phase, thereby further enhancing the temperature resistance of the ceramicized silicone rubber material. At the same time, by reasonably controlling the mass ratio of silicon powder and aluminum powder in the thermal compensator, it is beneficial to further enhance the dimensional stability of the ceramicized silicone rubber material.
[0044] According to some preferred embodiments, the shrinkage inhibitor is alumina fiber cotton; wherein the fiber diameter of the alumina fiber cotton is 3-4 microns (for example, 3 microns, 3.5 microns or 4 microns); and the flame retardant is aluminum hydroxide.
[0045] In the embodiment of the present invention, by adding alumina fiber cotton with a certain fiber diameter into the ceramic filler, the alumina fiber cotton can not only effectively inhibit the shrinkage of the ceramic silicone rubber material during the ceramicization process of methyl vinyl silicone rubber and the ceramic filler, but also the alumina fiber cotton has a certain temperature resistance. After rising to a certain temperature, the alumina fiber cotton can undergo a eutectic reaction with other components, thereby further enhancing the temperature resistance of the ceramic silicone rubber material.
[0046] It should be noted that the alumina content in the alumina fiber wool in the embodiment of the present invention is greater than 95%.
[0047] According to some preferred embodiments, the components of the porcelain-forming filler are as follows, measured in parts by weight: 40-80 parts of filler body (for example, 40 parts, 45 parts, 50 parts, 55 parts, 60 parts, 65 parts, 70 parts, 75 parts or 80 parts), 10-20 parts of solvent (for example, 10 parts, 15 parts or 20 parts), 0.5-5 parts of bonding aid (for example, 0.5 parts, 1 parts, 2 parts, 3 parts, 4 parts or 5 parts), 10-40 parts of thermal compensator (for example, 10 parts, 20 parts, 30 parts or 40 parts), 0.5-5 parts of shrinkage inhibitor (for example, 0.5 parts, 1 parts, 2 parts, 3 parts, 4 parts or 5 parts) and 5-13 parts of flame retardant (for example, 5 parts, 8 parts, 10 parts, 12 parts or 13 parts).
[0048] In the embodiment of the present invention, by reasonably controlling the raw materials of each component in the ceramic filler, it is beneficial to ceramicize the methyl vinyl silicone rubber and the ceramic filler to form a ceramic silicone rubber material with excellent mechanical properties, heat resistance and low shrinkage rate; for example, if the amount of bonding aid added is too low, it is not conducive to ensuring the good mechanical properties of the ceramic silicone rubber material, but if the amount of bonding aid added is too much, the thermal shrinkage rate of the ceramic silicone rubber material will be increased; if the amount of shrinkage inhibitor added is too low, it is not conducive to ensuring the low thermal shrinkage rate of the ceramic silicone rubber material, but if the amount of shrinkage inhibitor added is too much, the viscosity of the system will be increased, and the mechanical strength of the ceramic silicone rubber material will be reduced, and the ceramic silicone rubber material will be caused to warp after high temperature; at the same time, a certain amount of thermal compensating agent is beneficial to further enhance the temperature resistance of the ceramic silicone rubber material, but too much thermal compensating agent will increase the porosity of the material during the ceramicization process, thereby reducing the mechanical strength of the ceramic silicone rubber material and increasing the thermal shrinkage rate.
[0049] According to some preferred embodiments, the components of the porcelain-forming filler are as follows: 55-65 parts of filler body (for example, 55 parts, 58 parts, 60 parts, 62 parts or 65 parts), 15-18 parts of solvent (for example, 15 parts, 18 parts or 20 parts), 2-3 parts of bonding aid (for example, 2 parts, 2.5 parts or 3 parts), 15-25 parts of thermal compensator (for example, 15 parts, 18 parts, 20 parts or 25 parts), 2-3 parts of shrinkage inhibitor (for example, 2 parts, 2.5 parts or 3 parts) and 12-13 parts of flame retardant (for example, 12 parts, 12.5 parts or 13 parts).
[0050] Since the content of each component in the ceramic filler has a great influence on the performance of the ceramic silicone rubber material, the embodiment of the present invention further optimizes the content of each component in the ceramic filler, which is more conducive to the preparation of a ceramic silicone rubber material with better comprehensive properties (such as thermal shrinkage, mechanical strength, high temperature resistance, etc.).
[0051] It should be noted that the solvent, filler body, bonding aid, thermal compensator and flame retardant in the embodiment of the present invention are all in powder form. At the same time, in order to ensure that the ceramic filler has good sintering performance and prevent the ceramic filler from shrinking too much during the sintering process, the particle size of the above-mentioned powdered raw materials of the ceramic filler in the embodiment of the present invention is preferably 5-100 microns.
[0052] The embodiment of the present invention further provides a method for preparing the ceramic silicone rubber material as described in any one of the above items, the preparation method comprising the following steps:
[0053] (1) stirring and mixing the methyl vinyl silicone rubber and the porcelain-forming filler to obtain a mixed material;
[0054] (2) placing the mixed material in a mold for vulcanization reaction to obtain a flexible silicone rubber;
[0055] (3) placing the flexible silicone rubber in a muffle furnace for heating and ceramicization to obtain the ceramic silicone rubber.
[0056] In the embodiment of the present invention, the other ceramic fillers in the ceramic filler except the heat shrink agent need to be stirred and mixed at a higher mechanical speed (for example, 800-1000r / min), and then the speed is lowered (for example, 300-500r / min), and the heat shrink agent is added and mixed. This is not only beneficial to the uniformity between the components, but also can avoid the destruction of the heat shrink agent, so that it can better play the role of inhibiting thermal shrinkage.
[0057] It should be noted that, in the embodiments of the present invention, after the mixed material is prepared, the mixed material is placed in a mold, vacuum-degassed and extruded, so as to avoid air bubbles being trapped in the vulcanized silicone rubber.
[0058] According to some preferred embodiments, in step (2), the temperature of the vulcanization reaction is 22-24°C (for example, 22°C, 23°C or 24°C), and the time is 7-10 days (for example, 7 days, 8 days, 9 days or 10 days); or, the temperature of the vulcanization reaction is 40-42°C (for example, 40°C, 41°C or 42°C), and the time is 5-6h (for example, 5h, 5.5h or 6h).
[0059] In the embodiment of the present invention, by using the above-mentioned types of silicone rubber and catalyst, the molding temperature of the silicone rubber material can be reduced, and it can be molded at room temperature. It can be understood that as the temperature increases, it is conducive to accelerating the molding of the silicone rubber material.
[0060] In some preferred embodiments, in step (3), the heating temperature for ceramicization is 500-1600°C (for example, it can be 500°C, 600°C, 800°C, 1000°C, 1200°C, 1400°C or 1600°C), the heating rate is 10-30°C / min (for example, it can be 10°C / min, 15°C / min, 20°C / min, 25°C / min or 30°C / min), and the time is 30-90min (for example, it can be 30min, 40min, 50min, 60min, 70min, 80min or 90min).
[0061] In the embodiment of the present invention, by controlling the types and contents of methyl vinyl silicone rubber and ceramic fillers, it is beneficial for silicone rubber to have porcelain strength at a lower temperature (such as 500°C); for example, the flexible silicone rubber is heated from room temperature to 1600°C at a heating rate of 10°C / min. During the temperature increase, the silicone rubber undergoes thermal decomposition at 400°C to 500°C. At this temperature, after the low-melting point glass powder melts, its decomposition can be inhibited to a certain extent. At the same time, the shrinkage inhibitor and the bonding aid can play a role, thereby preventing the shrinkage rate of the ceramic silicone rubber material from being too large and ensuring the good mechanical properties of the ceramic silicone rubber material. When the temperature reaches 800-1000°C, the thermal compensator is oxidized to achieve weight gain, and the bonding aid undergoes a crystal transformation, thereby better bonding the other components together, ensuring the excellent mechanical properties of the ceramic silicone rubber material. When the temperature reaches above 1000°C, the products formed by the components in the ceramic filler can undergo a eutectic reaction, thereby forming a mullite phase with better heat resistance, thereby significantly enhancing the temperature resistance and mechanical properties of the ceramic silicone rubber material.
[0062] In summary, the present invention uses the above-mentioned types of silicone rubber and ceramic fillers to prepare ceramic silicone rubber, and the preparation process is simple. Not only can the silicone rubber be molded at room temperature without the need for professional equipment and secondary vulcanization, but the ceramic silicone rubber material can also be quickly ceramicized below 600°C. While having a low shrinkage rate (less than 12%) and good ceramic strength, it can also withstand high temperatures of up to 1600°C.
[0063] In order to more clearly illustrate the technical solution and advantages of the present invention, a ceramic silicone rubber material and a preparation method thereof are described in detail below through several embodiments.
[0064] In the following examples, the masses of methyl vinyl silicone rubber, catalyst, filler body, cosolvent, bonding agent, thermal compensator, shrinkage inhibitor and flame retardant are expressed in parts by weight.
[0065] Embodiment 1:
[0066] (1) 60 parts of filler body (alumina), 15 parts of co-solvent (low melting point glass powder), 2.5 parts of bonding agent (aluminum dihydrogen phosphate), 20 parts of thermal compensator (10:10 of silicon powder and aluminum powder) and 12.5 parts of flame retardant (aluminum hydroxide) are stirred at a speed of 1000 r / min for 30 minutes, then the speed is adjusted to 500 r / min, 2.5 parts of shrinkage inhibitor (alumina fiber cotton) are added and stirred for 30 minutes to obtain a ceramic filler; 100 parts of methyl vinyl silicone rubber (the platinum catalyst content is 0.5% of the total amount of methyl vinyl silicone rubber) and 150 parts of ceramic filler are manually or mechanically stirred and mixed to obtain a mixed material;
[0067] (2) The mixed material is transferred into a mold, vacuum degassed and extruded, and vulcanized at 23° C. for 8 days to obtain a flexible silicone rubber with a specification of 100×80×3 mm;
[0068] (3) The vulcanized flexible silicone rubber was cut into a size of 80×10×3 mm, placed in a muffle furnace and heated to 1600°C at a heating rate of 10°C / min and kept warm for 30 min-90 min. After cooling to room temperature (22-25°C), the ceramic silicone rubber material was obtained. The test results are shown in Table 1.
[0069] (4) The vulcanized flexible silicone rubber was cut into a size of 80×10×3 mm, placed in a muffle furnace and heated to 500°C, 600°C, 800°C, 1000°C, 1200°C, 1400°C and 1600°C at a heating rate of 10°C / min, and kept warm for 30 min. After cooling to room temperature (22-25°C), the ceramic silicone rubber material was obtained. The test results are shown in Table 2.
[0070] Embodiment 2:
[0071] (1) 40 parts of filler body (alumina), 15 parts of co-solvent (low melting point glass powder), 2.5 parts of bonding agent (aluminum dihydrogen phosphate), 20 parts of thermal compensator (10:10 of silicon powder and aluminum powder) and 7.5 parts of flame retardant (aluminum hydroxide) are stirred at a speed of 1000 r / min for 30 minutes, then the speed is adjusted to 500 r / min, 2.5 parts of shrinkage inhibitor (alumina fiber cotton) are added and stirred for 30 minutes to obtain a ceramic filler; 100 parts of methyl vinyl silicone rubber (the platinum catalyst content is 0.5% of the total amount of methyl vinyl silicone rubber) and 150 parts of ceramic filler are manually or mechanically stirred and mixed to obtain a mixed material;
[0072] (2) The mixed material is transferred into a mold, vacuum degassed and extruded, and vulcanized at 40° C. for 6 h to obtain a flexible silicone rubber with a specification of 100×80×3 mm;
[0073] (3) The vulcanized flexible silicone rubber was cut into a size of 80×10×3 mm, placed in a muffle furnace and heated to 600°C, 1000°C and 1600°C at a heating rate of 10°C / min and kept warm for 30 min respectively. After cooling to room temperature (22-25°C), the ceramic silicone rubber material was obtained. The test results are shown in Table 3.
[0074] Embodiment 3:
[0075] (1) 60 parts of filler body (alumina), 15 parts of cosolvent (low melting point glass powder), 0.5 parts of bonding agent (polyaluminum phosphate), 20 parts of thermal compensator (10:10 of silicon powder and aluminum powder) and 7.5 parts of flame retardant (aluminum hydroxide) are stirred at a speed of 1000 r / min for 30 minutes, then the speed is adjusted to 500 r / min, 2.5 parts of shrinkage inhibitor (alumina fiber cotton) are added and stirred for 30 minutes to obtain a ceramic filler; 100 parts of methyl vinyl silicone rubber (the platinum catalyst content is 0.5% of the total amount of methyl vinyl silicone rubber) and 150 parts of ceramic filler are manually or mechanically stirred and mixed to obtain a mixed material;
[0076] (2) The mixed material is transferred into a mold, vacuum degassed and extruded, and vulcanized at 23° C. for 10 days to obtain a flexible silicone rubber with a specification of 100×80×3 mm;
[0077] (3) The vulcanized flexible silicone rubber was cut into a size of 80×10×3 mm, placed in a muffle furnace and heated to 600°C, 1000°C and 1600°C at a heating rate of 10°C / min and kept warm for 30 min respectively. After cooling to room temperature (22-25°C), the ceramic silicone rubber material was obtained. The test results are shown in Table 4.
[0078] Embodiment 4:
[0079] (1) 60 parts of filler body (alumina), 15 parts of cosolvent (low melting point glass powder), 2.5 parts of bonding agent (aluminum metaphosphate), 20 parts of thermal compensator (10:10 of silicon powder and aluminum powder) and 12.5 parts of flame retardant (aluminum hydroxide) are stirred at a speed of 1000 r / min for 30 minutes, then the speed is adjusted to 500 r / min, 2.5 parts of shrinkage inhibitor (alumina fiber cotton) are added and stirred for 30 minutes to obtain a ceramic filler; 100 parts of methyl vinyl silicone rubber (the platinum catalyst content is 0.5% of the total amount of methyl vinyl silicone rubber) and 100 parts of ceramic filler are manually or mechanically stirred and mixed to obtain a mixed material;
[0080] (2) The mixed material is transferred into a mold, vacuum degassed and extruded, and vulcanized at 23° C. for 8 days to obtain a flexible silicone rubber with a specification of 100×80×3 mm;
[0081] (3) The vulcanized flexible silicone rubber was cut into a size of 80×10×3 mm, placed in a muffle furnace and heated to 600°C, 1000°C and 1600°C at a heating rate of 10°C / min and kept warm for 30 min respectively. After cooling to room temperature (22-25°C), the ceramic silicone rubber material was obtained. The test results are shown in Table 5.
[0082] Embodiment 5:
[0083] (1) 60 parts of filler body (alumina), 15 parts of co-solvent (low melting point glass powder), 2.5 parts of bonding agent (aluminum dihydrogen phosphate), 20 parts of thermal compensator (10:10 of silicon powder and aluminum powder) and 12.5 parts of flame retardant (aluminum hydroxide) are stirred at a speed of 1000 r / min for 30 minutes, then the speed is adjusted to 500 r / min, 2.5 parts of shrinkage inhibitor (alumina fiber cotton) are added and stirred for 30 minutes to obtain a ceramic filler; 100 parts of methyl vinyl silicone rubber (the platinum catalyst content is 0.5% of the total amount of methyl vinyl silicone rubber) and 200 parts of ceramic filler are manually or mechanically stirred and mixed to obtain a mixed material;
[0084] (2) The mixed material is transferred into a mold, vacuum degassed and extruded, and vulcanized at 23° C. for 8 days to obtain a flexible silicone rubber with a specification of 100×80×3 mm;
[0085] (3) The vulcanized flexible silicone rubber was cut into a size of 80×10×3 mm, placed in a muffle furnace and heated to 600°C, 1000°C and 1600°C at a heating rate of 10°C / min and kept warm for 30 min respectively. After cooling to room temperature (22-25°C), the ceramic silicone rubber material was obtained. The test results are shown in Table 6.
[0086] Embodiment 6:
[0087] (1) 60 parts of filler body (alumina), 15 parts of co-solvent (low melting point glass powder), 2.5 parts of bonding agent (aluminum dihydrogen phosphate), 20 parts of thermal compensator (10:10 of silicon powder and aluminum powder) and 7.5 parts of flame retardant (aluminum hydroxide) are stirred at a speed of 1000 r / min for 30 minutes, then the speed is adjusted to 500 r / min, 2.5 parts of shrinkage inhibitor (alumina fiber cotton) are added and stirred for 30 minutes to obtain a ceramic filler; 100 parts of methyl vinyl silicone rubber (the platinum catalyst content is 0.5% of the total amount of methyl vinyl silicone rubber) and 150 parts of ceramic filler are manually or mechanically stirred and mixed to obtain a mixed material;
[0088] (2) The mixed material is transferred into a mold, vacuum degassed and extruded, and vulcanized at 40° C. for 6 h to obtain a flexible silicone rubber with a specification of 100×80×3 mm;
[0089] (3) The vulcanized flexible silicone rubber was cut into a size of 80×10×3 mm, placed in a muffle furnace and heated to 1600°C at a heating rate of 10°C / min, 20°C / min and 30°C / min, respectively, and kept warm for 30 min, respectively. After cooling to room temperature (22-25°C), the ceramic silicone rubber material was obtained. The test results are shown in Table 7.
[0090] Embodiment 7:
[0091] Example 7 is basically the same as Example 1, except that in step (1), the mass ratio of methyl vinyl silicone rubber to ceramic filler is 100:220.
[0092] Embodiment 8:
[0093] Example 8 is basically the same as Example 1, except that in step (1), the amount of the bonding aid (aluminum dihydrogen phosphate) added is 6 parts.
[0094] Embodiment 9:
[0095] Example 9 is basically the same as Example 1, except that in step (1), the amount of shrinkage inhibitor (alumina fiber cotton) added is 6 parts.
[0096] Embodiment 10:
[0097] Example 10 is basically the same as Example 1, except that in step (1), the amount of thermal compensator (silicon powder) added is 30 parts.
[0098] Comparative Example 1:
[0099] Comparative Example 1 is substantially the same as Example 1, except that in step (1), the ceramic filler does not contain a bonding aid (aluminum dihydrogen phosphate).
[0100] Comparative Example 2:
[0101] Comparative Example 2 is substantially the same as Example 1, except that in step (1), the porcelain-forming filler does not contain a shrinkage inhibitor (alumina fiber wool).
[0102] Comparative Example 3:
[0103] Comparative Example 3 is substantially the same as Example 1, except that in step (1), the ceramic filler does not contain thermal compensating agent (silicon powder and aluminum powder).
[0104] Comparative Example 4:
[0105] Comparative Example 4 is substantially the same as Example 1, except that in step (1), the filler body is replaced with sericite.
[0106] The ceramic silicone rubber materials prepared in Examples 1 to 10 and Comparative Examples 1 to 4 (hereinafter referred to as samples) were subjected to performance tests and their macroscopic appearance changes were observed. The test results are as follows: Figures 1 to 7 and as shown in Tables 1 to 8.
[0107] Specifically, the mass loss rate (m a ) refers to the change ratio of the weight m1 of the sample after high temperature heat treatment to the weight m0 before heat treatment;
[0108] Linear shrinkage (l a ) refers to the change ratio of the length l1 of the sample after high-temperature heat treatment relative to the size l0 before heat treatment. The sample size is 80mm×10mm×3mm. The calculation formulas for the two are as follows:
[0109]
[0110] The bending strength of the sintered samples was tested according to the national standard GB / T 9341-2008, and the bending strength of the samples after heat treatment at different temperatures was tested using an INSTRON-5969 universal testing machine, with a loading rate of 2 mm / min.
[0111] The calculation formula for bending strength is:
[0112]
[0113] In the formula,
[0114] σ f ——Bending strength, unit: MPa;
[0115] F——pressure, unit N;
[0116] L——span of the sample, in mm;
[0117] b——the width of the sample, in mm;
[0118] h is the thickness of the sample, in mm.
[0119] Table 1
[0120]
[0121] Table 2
[0122]
[0123]
[0124] Table 3
[0125]
[0126] Table 4
[0127]
[0128] Table 5
[0129]
[0130] Table 6
[0131]
[0132]
[0133] Table 7
[0134]
[0135] Table 8
[0136]
[0137] Note: The heating rate is 10℃ / min and the holding time at 1600℃ is 30min.
[0138] From Tables 1 to 8 and Figures 1 to 8 It can be seen that, compared with the comparative example, the ceramic silicone rubber prepared in the embodiment of the present invention can be ceramicized at a temperature lower than 600°C, and the ceramicized silicone rubber material still has good mechanical strength (i.e., bending strength). At the same time, due to the reasonable selection of ceramic fillers and the control of the added amount, the ceramic silicone rubber material prepared in the embodiment of the present invention has a lower thermal shrinkage rate, a higher temperature resistance and a higher mechanical strength.
[0139] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A ceramic silicone rubber material, characterized in that: It is composed of methyl vinyl silicone rubber and ceramic filler; wherein the ceramic filler is composed of a filler body, a solvent, a bonding aid, a thermal compensator, a shrinkage inhibitor and a flame retardant.
2. The material according to claim 1, characterized in that The methyl vinyl silicone rubber contains a platinum catalyst, and the content of the platinum catalyst is 0.5-1.0% of the total amount of the methyl vinyl silicone rubber; and / or The viscosity of the methyl vinyl silicone rubber is 5000-20000 mPa·s, and the mass ratio of the methyl vinyl silicone rubber to the ceramic filler is 100:(100-200).
3. The material according to claim 1, characterized in that The filler is mainly aluminum oxide, and the flux is low-melting-point glass powder; and / or The bonding aid is at least one of aluminum dihydrogen phosphate, aluminum polyphosphate or aluminum metaphosphate.
4. The material according to claim 1, characterized in that The thermal compensating agent is composed of silicon powder and aluminum powder; wherein the mass ratio of silicon powder to aluminum powder is (5-20): (5-20).
5. The material according to claim 1, characterized in that The shrinkage inhibitor is alumina fiber cotton; wherein the fiber diameter of the alumina fiber cotton is 3-4 microns; and / or The flame retardant is aluminum hydroxide.
6. The material according to claim 1, characterized in that The composition of the ceramic filler is as follows, in parts by weight: 40-80 parts of filler body, 10-20 parts of cosolvent, 0.5-5 parts of bonding aid, 10-40 parts of thermal compensator, 0.5-5 parts of shrinkage inhibitor and 5-13 parts of flame retardant.
7. The material according to claim 6, characterized in that The components of the porcelain-forming filler are as follows: 55-65 parts of filler body, 15-18 parts of co-solvent, 2-3 parts of bonding aid, 15-25 parts of thermal compensator, 2-3 parts of shrinkage inhibitor and 12-13 parts of flame retardant.
8. The method for preparing a ceramic silicone rubber material according to any one of claims 1 to 7, characterized in that: The preparation method comprises the following steps: (1) stirring and mixing the methyl vinyl silicone rubber and the porcelain-forming filler to obtain a mixed material; (2) placing the mixed material in a mold for vulcanization reaction to obtain a flexible silicone rubber; (3) placing the flexible silicone rubber in a muffle furnace for heating and ceramicization to obtain the ceramic silicone rubber.
9. The preparation method according to claim 8, characterized in that: In step (2), the temperature of the sulfurization reaction is 22-24° C. and the time is 7-10 days; or The temperature of the vulcanization reaction is 40-42° C. and the time is 5-6 hours.
10. The preparation method according to claim 8, characterized in that: In step (3), the heating and ceramicizing temperature is 500-1600°C, the heating rate is 10-30°C / min, and the time is 30-90min.
Citation Information
Patent Citations
Coatable ceramic silicone rubber and preparation method therefor
CN105623273A
Preparation method of ceramic silicon rubber composite material used for fire-resistant insulated cable
CN105647190A
Superhard amorphous state ceramic silica gel and preparation method thereof as well as composition used for preparing superhard amorphous state ceramic silica gel
CN106986655A
Expansible ceramic silicone rubber composite material and preparation method thereof
CN107760038A
Waterproof anti-aging ceramicized silicon rubber material and preparation method and application thereof
CN108948743A