Method for preparing 2, 2-bis (4-aminocyclohexyl) propane by hydroamination of hydrogenated bisphenol A

Ni-B/SiO2 catalyst prepared by one-step continuous process and ammonia distillation method solves the high cost and pollution problems in the bisphenol A hydroaminization process, and achieves the efficient preparation of 2,2-bis(4-aminocyclohexyl ) The high catalytic activity and stability of propane reduces process costs and pollution.

CN119019262APending Publication Date: 2024-11-26JIANGSU QINGQUAN CHEM CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411110649.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

In the prior art, the process of preparing 2,2-bis(4-aminocyclohexyl)propane by hydrogenation of bisphenol A has high cost and environmental pollution problems. Traditional precious metal catalysts are costly and are not suitable for industrial applications. Non-precious metal catalysts are In the intermittent kettle process, the large emission of hydrogen and ammonia leads to high production costs and high pollution.

Method used

The Ni-B/SiO2 catalyst prepared by the ammonia vaporization method is adopted to carry out the hydrogenated bisphenol A and liquid ammonia and hydrogen through a fixed bed reactor. The active component of the catalyst Ni and the support SiO2 are used. The nickel silicate structure of phyllum is formed, and combined with alkali metal additives to inhibit the agglomeration of metal Ni and the coking of the catalyst surface to achieve efficient preparation of 2,2-bis(4-aminocyclohexyl)propane.

Benefits of technology

High catalytic activity and stability are achieved, process costs are reduced, pollution is reduced, operation is simple, catalyst loss is low, and excess hydrogen and liquid ammonia can be recovered, reducing process costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004992087180000061
    Figure BDA0004992087180000061
  • Figure BDA0004992087180000081
    Figure BDA0004992087180000081
  • Figure BDA0004992087180000091
    Figure BDA0004992087180000091
Patent Text Reader

Abstract

The invention provides a method for preparing 2, 2-bis (4-aminocyclohexyl) propane through hydroamination of hydrogenated bisphenol A. The method comprises the following steps: with a fixed bed reactor as a reaction place, carrying out a hydroamination reaction on a hydrogenated bisphenol A solution, liquid ammonia and hydrogen under a catalyst and preset reaction conditions to prepare 2, 2-bis (4-aminocyclohexyl) propane, with the catalyst being a Ni-B / SiO2 catalyst prepared by an ammonia distillation method, the preset reaction conditions comprise that the hydrogen pressure is 8-12 MPa, the reaction temperature is 180-240 DEG C, and the volume space velocity is 0.1-0.6 h <-1 >; the Ni-B / SiO2 catalyst comprises an active component Ni, an auxiliary agent B and a carrier SiO2, wherein a nickel silicate structure is formed between the active component Ni and the carrier SiO2. According to the method provided by the invention, hydrogenated bisphenol A can be used for continuously preparing 2, 2-bis-(4-aminocyclohexyl) propane through one-step hydroamination, the continuous process has the advantages of simplicity in operation, high productivity, lower catalyst loss and the like, and the adopted catalyst has the advantages of high catalytic activity and good stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of fine chemicals, and in particular relates to a method for preparing 2,2-bis(4-aminocyclohexyl)propane by hydrogenating bisphenol A. Background Art

[0002] As a monomer for preparing new polyimides, 2,2-bis-(4-aminocyclohexyl)propane has the advantages of relatively flexible polymer chains, low glass transition temperature and high crystallinity. The preparation of 2,2-bis-(4-aminocyclohexyl)propane by hydrogenation of bisphenol A requires a "dehydrogenation-imidization-hydrogenation" process, so the catalyst for this reaction must have good dehydrogenation / hydrogenation functions at the same time. Pt, Pd and other traditional precious metal hydrogenation / dehydrogenation catalysts are not suitable for widespread use due to their high cost. Non-precious metals Ni and Co have stronger oxygen affinity and are cheaper than precious metal catalysts, so they are more suitable for industrialization.

[0003] Patent US3551485 reports a method for preparing 2,2-bis-(4-aminocyclohexyl)alkane by hydroamination of 2,2-bis-(4-hydroxycyclohexyl)alkane in a batch process using a Co-based catalyst supported by a silicon oxide or aluminum oxide carrier. The molar ratio of 2,2-bis-(4-hydroxycyclohexyl)alkane to ammonia is 1 / 3 to 1 / 6, the hydrogen pressure is 10 to 40 MPa, the reaction temperature is 150 to 200°C, and the yield of 2,2-bis-(4-aminocyclohexyl)alkane is 92.7%. This process is an intermittent batch production process. After the reaction is completed, it needs to go through cooling, pressure relief, and discharge processes, resulting in large amounts of hydrogen and ammonia being discharged. The process has high production costs and severe environmental pollution. Summary of the invention

[0004] The object of the present invention is to provide a process for continuously preparing 2,2-bis-(4-aminocyclohexyl)propane by hydrogenating bisphenol A through a one-step hydroamination, and the catalyst used has the advantages of high catalytic activity and good stability.

[0005] In order to achieve the above object, the present invention provides a method for preparing 2,2-bis(4-aminocyclohexyl)propane by hydroamination of hydrogenated bisphenol A. The method comprises: using a fixed bed reactor as a reaction site, and under a catalyst and preset reaction conditions, allowing a hydrogenated bisphenol A solution, liquid ammonia and hydrogen to undergo hydroamination reaction to prepare 2,2-bis(4-aminocyclohexyl)propane, wherein the catalyst is a Ni-B / SiO2 catalyst prepared by an ammonia evaporation method, and the preset reaction conditions include: a hydrogen pressure of 8 to 12 MPa, a reaction temperature of 180 to 240° C., and a volume space velocity of 0.1 to 0.6 h -1; Wherein, the Ni-B / SiO2 catalyst includes an active component Ni, an additive B and a carrier SiO2, and a nickel sheet silicate structure is formed between the active component Ni and the carrier SiO2. Based on the total weight of the catalyst as 100%, the mass percentage of the active component Ni is 10 to 25%.

[0006] In a specific embodiment, the auxiliary agent B is an oxide of an auxiliary element, and the auxiliary element is selected from one or a combination of at least two of K, Na, Ce, Ca, Fe, La, Mg, and Ba. Based on the total weight of the catalyst as 100%, the mass percentage of the auxiliary element is 2 to 6%.

[0007] In a specific embodiment, it is characterized in that the ammonia evaporation method is specifically as follows: first, nickel nitrate and metal hydrochloric acid of auxiliary elements are prepared into a solution, after ammonia water is added for complexation, silica sol is added at 20-60°C, and the dropping time is controlled to be 0.5h-4h. After the dropping is completed, the temperature is kept for 1h-4h, and then the temperature is increased to 60-100°C to evaporate ammonia until the mother liquor pH = 6, and the ammonia evaporation is stopped. The feed liquid after ammonia evaporation is filtered, washed, dried, and roasted to obtain the catalyst.

[0008] In a specific embodiment, in the ammonia evaporation method, the drying temperature is 100-150° C., and the drying time is 6 h to 15 h.

[0009] In a specific embodiment, in the ammonia distillation method, the roasting temperature is 500-800° C. and the roasting time is 2-8 hours.

[0010] In a specific embodiment, the method further comprises reducing the Ni-B / SiO2 catalyst before the hydroamination reaction, wherein the reduction of the Ni-B / SiO2 catalyst is specifically as follows: using a hydrogen-nitrogen mixed gas as a reducing agent, a reduction temperature of 400-700° C., and a reduction time of 2 h to 8 h, wherein the volume percentage of hydrogen in the hydrogen-nitrogen mixed gas is 10-90%, and the hydrogen volume space velocity is 50-300 h -1 .

[0011] In a specific embodiment, the hydrogenated bisphenol A solution includes hydrogenated bisphenol A and a solvent, and the solvent is one of dioxane, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, and tetrahydrofuran.

[0012] In a specific embodiment, based on the total weight of the hydrogenated bisphenol A solution being 100%, the mass fraction of the hydrogenated bisphenol A is 10-30 wt %.

[0013] In a specific embodiment, the molar ratio of hydrogenated bisphenol A to liquid ammonia is 1:(4-10), and the molar ratio of hydrogenated bisphenol A to H2 is 1:(2-6).

[0014] In a specific embodiment, the reaction temperature is 220-240°C.

[0015] The beneficial effects of the present invention include at least:

[0016] 1. The method for preparing 2,2-bis(4-aminocyclohexyl)propane by hydroamination of hydrogenated bisphenol A provided by the present invention, using a fixed bed reactor as reaction conditions, under a catalyst and preset reaction conditions, hydrogenated bisphenol A solution, liquid ammonia and hydrogen undergo hydroamination reaction to prepare 2,2-bis(4-aminocyclohexyl)propane, the catalyst is a Ni-B / SiO2 catalyst prepared by an ammonia evaporation method, and a nickel phyllosilicate structure is formed between the active component Ni and the carrier SiO2; thus, on the one hand, since the nickel phyllosilicate structure is formed between Ni and the carrier SiO2, the active component Ni is highly dispersed, and Ni is not easy to agglomerate during the reaction; on the other hand, the addition of the alkaline metal additive, due to the interaction between the alkaline metal additive and the Ni metal, further inhibits the agglomeration of the metal Ni and the coking of the catalyst surface, and reduces the condensation side reaction, the target product 2,2-bis-(4-aminocyclohexyl)propane has a high yield and good catalyst stability.

[0017] 2. The method for preparing 2,2-bis(4-aminocyclohexyl)propane by hydroamination of hydrogenated bisphenol A provided by the present invention can use a fixed bed reactor as a reaction site to achieve a continuous hydroamination reaction. Compared with the intermittent reactor production process in the prior art, the continuous process has the advantages of simple operation, large production capacity and low catalyst loss. At the same time, the continuous process can achieve continuous feeding and discharging, avoiding further reaction of the product causing a decrease in primary amine selectivity, and the excess hydrogen and liquid ammonia in the reaction can be recovered and reused, thereby reducing process costs and reducing pollution. DETAILED DESCRIPTION

[0018] The present invention is described in detail below with reference to the embodiments.

[0019] The invention provides a method for preparing 2,2-bis(4-aminocyclohexyl)propane by hydroamination of hydrogenated bisphenol A. The method comprises the following steps: a hydrogenated bisphenol A solution and liquid ammonia are pumped into a fixed bed reactor by a plunger pump; and under a catalyst and preset reaction conditions, the hydrogenated bisphenol A solution, liquid ammonia and hydrogen undergo a hydroamination reaction to prepare 2,2-bis(4-aminocyclohexyl)propane.

[0020] In the present invention, the preset reaction conditions include: hydrogen pressure of 8MPa-12MPa, reaction temperature of 180-240°C, volume space velocity of 0.1h -1 ~0.6h -1 .

[0021] Preferably, the hydrogen pressure is 10-12 MPa, the reaction temperature is 220-240°C, and the volume space velocity is 0.1 h -1 ~0.3h -1 .

[0022] Preferably, the hydrogenated bisphenol A solution comprises hydrogenated bisphenol A and a solvent, and the solvent is one of dioxane, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, and tetrahydrofuran.

[0023] Preferably, based on the total weight of the hydrogenated bisphenol A solution being 100%, the mass fraction of the hydrogenated bisphenol A is 10-30 wt %.

[0024] Preferably, the molar ratio of hydrogenated bisphenol A to liquid ammonia is 1:(4-10), and the molar ratio of hydrogenated bisphenol A to H2 is 1:(2-6).

[0025] In the present invention, the catalyst is a Ni-B / SiO2 catalyst prepared by an ammonia evaporation method, comprising an active component Ni, an additive B and a carrier SiO2, wherein a nickel sheet silicate structure is formed between the active component Ni and the carrier SiO2, and the mass percentage of the active component Ni is 10 to 25% based on the total weight of the catalyst being 100%.

[0026] Preferably, the auxiliary agent B is an oxide of an auxiliary element, and the auxiliary element is selected from one or a combination of at least two of K, Na, Ce, Ca, Fe, La, Mg, and Ba.

[0027] That is, the catalyst can also be expressed as Ni-MeOx / SiO2, where Me is selected from one or a combination of at least two of K, Na, Ce, Ca, Fe, La, Mg, and Ba.

[0028] Preferably, based on 100% of the total weight of the catalyst, the mass percentage of the auxiliary element is 2-6%.

[0029] That is, based on the total weight of the catalyst being 100%, the mass percentage of Me in the catalyst is 2-6%.

[0030] It can be understood here that the mass percentage of metal elements (promoter elements) in the catalyst is 2-6%, that is, the mass percentage of K, Na, Ce, Ca, Fe, La, Mg, and Ba is 2-6%.

[0031] More preferably, the auxiliary element is selected from one of Fe, Ca, Ce and Ba.

[0032] That is, the catalyst is Ni-MeOx / SiO2, wherein Me is selected from one of Fe, Ca, Ce and Ba.

[0033] More preferably, the additive B is an oxide of an additive element, the additive element is Fe, and the catalyst is Ni-FeO x / SiO2 catalyst.

[0034] Preferably, the ammonia evaporation method is specifically as follows: first, nickel nitrate and a metal salt of an auxiliary element are prepared into a solution, ammonia water is added dropwise for complexation, and then silica sol is added dropwise at 20 to 60° C., and the dropping time is controlled to be 0.5 h to 4 h. After the dropping is completed, the temperature is kept for 1 h to 4 h, and then the temperature is raised to 60 to 100° C. to evaporate ammonia, and the ammonia evaporation is stopped when the pH of the mother liquor is 6. The feed liquid after ammonia evaporation is filtered, washed, dried, and calcined to obtain the catalyst.

[0035] Preferably, in the ammonia evaporation method, the drying temperature is 100-150° C., and the drying time is 6 h to 15 h; the roasting temperature is 500-800° C., and the roasting time is 2 h to 8 h.

[0036] More preferably, the calcination temperature is 500-600° C., and the calcination time is 6 h-8 h.

[0037] Preferably, the method further comprises reducing the Ni-B / SiO2 catalyst before the hydroamination reaction, wherein the reduction of the Ni-B / SiO2 catalyst is specifically as follows: using a hydrogen-nitrogen mixed gas as a reducing agent, a reduction temperature of 400-700° C., and a reduction time of 2 h to 8 h, wherein the volume percentage of hydrogen in the hydrogen-nitrogen mixed gas is 10-90%, and the hydrogen volume space velocity is 50 h -1 ~300h -1 .

[0038] Example 1

[0039] Weigh 45.31g of Ni(NO3)2·6H2O and 13.24g of Fe(NO3)3·9H2O in a 1000mL round-bottom flask, add 200.0g of purified water to dissolve, add 165.0g of 25wt% ammonia water dropwise while stirring, stir for 30min at room temperature, slowly add 200.0g of silica sol solution (25wt% SiO2) dropwise at 20-60°C for 2h, keep warm for 3h after the addition is completed, heat to 60-100°C to evaporate ammonia, stop heating when the pH value of the mixture drops to 6.0, filter, wash with deionized water several times, dry at 120°C for 12h, and calcine at 600°C for 6h to obtain Ni-FeO with a Ni mass fraction of 15% and a Fe mass fraction of 3.0%. x / SiO2 catalyst, denoted as 15%Ni-3%FeO x / SiO2 catalyst.

[0040] Catalyst activity evaluation:

[0041] Specifically, the 15% Ni-3% FeO prepared in Example 1 x / SiO2 catalyst is used for hydrogenation of bisphenol A to prepare 2,2-bis(4-aminocyclohexyl)propane.

[0042] Preparation of hydrogenated bisphenol A solution: the mass fraction of hydrogenated bisphenol A in the hydrogenated bisphenol A solution is 15%, and the solvent in the hydrogenated bisphenol A solution is tetrahydrofuran.

[0043] Reaction site: fixed bed reactor, the reaction tube is a quartz tube with an inner diameter of 13 mm and a length of 60 cm.

[0044] The evaluation process is as follows: the powder catalyst prepared in the example is pressed into tablets, crushed, and 6.0 g of the catalyst with a size of 20 to 40 mesh is selected and loaded into a fixed bed reactor for reaction. The temperature is first raised to 550°C, reduced by a hydrogen / nitrogen mixed gas for 6 h, cooled to the reaction temperature, and heated to 400°C at a volume space velocity of 0.3 h -1 The catalyst was evaluated under the following conditions, wherein the volume ratio of hydrogen to nitrogen in the hydrogen / nitrogen mixture was 1:2 and the hydrogen space velocity was 300 h -1 .

[0045] It should be noted that the catalyst bed temperature (ie, reaction temperature) was controlled by programmed temperature rise: the test temperature interval was 2°C / min, and each test temperature point was maintained for 1 hour.

[0046] The catalytic activity of the catalyst prepared in Example 1 under different reaction conditions is shown in Table 1.

[0047] Table 1 15%Ni-3%FeO x Catalytic activity of SiO2 catalyst under different reaction conditions

[0048] Reaction temperature / ℃ Hydrogen pressure / MPa HBPA / Liquid Ammonia <![CDATA[H2 / HBPA]]> Conversion rate / % Selectivity% 180 12 1 / 8 6 84.21 90.44 200 12 1 / 8 6 91.55 92.82 220 12 1 / 8 6 94.71 94.28 240 12 1 / 8 6 96.24 92.51

[0049] It can be seen from Table 1 that under the same hydrogen pressure, HBPA / ammonia and H2 / HBPA, as the reaction temperature increases, the conversion rate of hydrogenated bisphenol A gradually increases, while the selectivity of 2,2-bis(4-aminocyclohexyl)propane first increases and then decreases.

[0050] Preferably, the reaction temperature is 220-240°C.

[0051] Example 2

[0052] Example 2 is the same as Example 1, except that when the catalyst is prepared by ammonia evaporation, the salt of the auxiliary agent added is 5.67 g of Ce(NO3)3·6H2O, and the prepared catalyst is Ni-CeO x / SiO2 catalyst, wherein the mass fraction of Ni is 15.0% and the mass fraction of Ce is 3.0%, recorded as 15%Ni-3%CeO x / SiO2.

[0053] According to the catalyst activity evaluation method provided in Example 1, the catalytic activity of the catalyst prepared in Example 2 was evaluated. The catalytic activity evaluation results are shown in Table 2.

[0054] Example 3

[0055] Example 3 is the same as Example 1, except that when the catalyst is prepared by the ammonia evaporation method, the salt of the auxiliary agent added is 3.49 g of Ba(NO3)2, and the prepared catalyst is Ni-BaO x / SiO2 catalyst, wherein the mass fraction of Ni is 15.0% and the mass fraction of Ba is 3.0%, recorded as 15%Ni-3%BaO x / SiO2.

[0056] According to the catalyst activity evaluation method provided in Example 1, the catalytic activity of the catalyst prepared in Example 3 was evaluated. The catalytic activity evaluation results are shown in Table 2.

[0057] Example 4

[0058] Example 4 is the same as Example 1, except that when the catalyst is prepared by ammonia evaporation, the salt of the auxiliary agent added is 10.81 g of Ca(NO3)2·4H2O, and the catalyst prepared is Ni-CaO x / SiO2 catalyst, wherein the mass fraction of Ni is 15.0% and the mass fraction of Ca is 3.0%, recorded as 15%Ni-3%CaO x / SiO2.

[0059] According to the catalyst activity evaluation method provided in Example 1, the catalytic activity of the catalyst prepared in Example 4 was evaluated. The catalytic activity evaluation results are shown in Table 2.

[0060] Table 2 Catalytic activity of catalysts prepared in Example 1 to Example 4 under different reaction conditions

[0061]

[0062] It can be seen from Table 2 that the catalysts prepared with different metal oxides as additives have higher conversion rates and selectivities when applied to the process of preparing 2,2-bis-(4-aminocyclohexyl)propane by hydrogenation of bisphenol A. x When used as an additive, its synergistic effect is better than that of other metal oxides.

[0063] Example 5

[0064] Example 5 is the same as Example 1, except that when the catalyst is prepared by the ammonia evaporation method, the masses of the Ni salt and the Fe salt added are different. Specifically: Example 5 weighs 28.15 g of Ni(NO3)2·6H2O and 8.23 ​​g of Fe(NO3)3·9H2O in a 1000 mL round-bottom flask to prepare a Ni-FeO catalyst. x / SiO2 catalyst, in which the mass fraction of Ni is 10.0% and the mass fraction of Fe is 2.0%, recorded as 10%Ni-2%FeO x / SiO2.

[0065] According to the catalyst activity evaluation method provided in Example 1, the catalytic activity of the catalyst prepared in Example 5 was evaluated. The catalytic activity evaluation results are shown in Table 3.

[0066] Table 3 10%Ni-2%FeO x Catalytic activity of SiO2 catalyst under different reaction conditions

[0067] Reaction temperature / ℃ Hydrogen pressure / MPa HBPA / Liquid Ammonia <![CDATA[H2 / HBPA]]> Conversion rate / % Selectivity% 220 12 1 / 8 6 92.29 92.54 220 10 1 / 8 6 92.15 92.65 220 8 1 / 8 6 91.99 91.57

[0068] It can be seen from Table 3 that when the reaction temperature, HBPA / ammonia and H2 / HBPA are the same, with the increase of hydrogen pressure, the conversion rate of hydrogenated bisphenol A gradually increases, while the selectivity of 2,2-bis(4-aminocyclohexyl)propane first increases and then slightly decreases. Preferably, the hydrogen pressure is 10 MPa.

[0069] Example 6

[0070] Example 6 is the same as Example 1, except that when the catalyst is prepared by the ammonia evaporation method, the masses of the Ni salt and the Fe salt added are different. Specifically: Example 6 weighs 65.19 g of Ni(NO3)2·6H2O and 19.05 g of Fe(NO3)3·9H2O in a 1000 mL round-bottom flask to prepare a Ni-FeO catalyst. x / SiO2 catalyst, in which the mass fraction of Ni is 20.0% and the mass fraction of Fe is 4.0%, recorded as 20%Ni-4%FeO x / SiO2, the corresponding Fe / Ni ratio is 1 / 5.

[0071] According to the catalyst activity evaluation method provided in Example 1, the catalytic activity of the catalyst prepared in Example 6 was evaluated. The catalytic activity evaluation results are shown in Table 4.

[0072] Table 4 20%Ni-4%FeO x Catalytic activity of SiO2 catalyst under different reaction conditions

[0073] Reaction temperature / ℃ Hydrogen pressure / MPa HBPA / Liquid Ammonia <![CDATA[H2 / HBPA]]> Conversion rate / % Selectivity% 220 12 1 / 10 6 94.54 94.57 220 12 1 / 8 6 95.19 94.19 220 12 1 / 6 6 95.67 93.91 220 12 1 / 4 6 96.07 92.61

[0074] It can be seen from Table 4 that under the same reaction temperature, hydrogen pressure and H2 / HBPA, as the HBPA / liquid ammonia molar ratio increases, the conversion rate of hydrogenated bisphenol A gradually increases, while the selectivity of 2,2-bis(4-aminocyclohexyl)propane gradually decreases.

[0075] Example 7

[0076] Example 7 is the same as Example 1, except that when the catalyst is prepared by the ammonia evaporation method, the masses of the Ni salt and the Fe salt added are different. Specifically: Example 7 weighs 88.47 g of Ni(NO3)2·6H2O and 25.86 g of Fe(NO3)3·9H2O in a 1000 mL round-bottom flask to prepare a Ni-FeO catalyst. x / SiO2 catalyst, in which the mass fraction of Ni is 25.0% and the mass fraction of Fe is 5.0%, recorded as 25%Ni-5%FeO x / SiO2, the corresponding Fe / Ni ratio is 1 / 5.

[0077] According to the catalyst activity evaluation method provided in Example 1, the catalytic activity of the catalyst prepared in Example 7 was evaluated. The catalytic activity evaluation results are shown in Table 5.

[0078] Table 5 25%Ni-5%FeO x Catalytic activity of SiO2 catalyst under different reaction conditions

[0079] Reaction temperature / ℃ Hydrogen pressure / MPa HBPA / Liquid Ammonia <![CDATA[H2 / HBPA]]> Conversion rate / % Selectivity% 220 12 1 / 8 6 95.98 93.12 220 12 1 / 8 4 96.09 92.88 220 12 1 / 8 2 96.05 92.30

[0080] It can be seen from Table 5 that under the same reaction temperature, hydrogen pressure and HBPA / liquid ammonia, with the increase of H2 / HBPA molar ratio, the conversion of hydrogenated bisphenol A first increases and then slightly decreases, with little overall difference, while the selectivity of 2,2-bis(4-aminocyclohexyl)propane gradually increases.

[0081] Comparing the experimental results in Table 1, Table 3, Table 4 and Table 5, it can be seen that with the increase of the mass fraction of metal, the primary amine yield first increases and then decreases. -1 The reaction conditions were: reaction pressure 10 MPa, HBPA / ammonia = 1 / 6, reaction temperature 220°C, and H2 / HBPA molar ratio = 4 / 1.

[0082] Example 8

[0083] Example 8 is the same as Example 1, except that when the catalyst is prepared by the ammonia evaporation method, the masses of the Ni salt and the Fe salt added are different. Specifically: Example 8 weighs 66.06 g of Ni(NO3)2·6H2O and 24.13 g of Fe(NO3)3·9H2O in a 1000 mL round-bottom flask to prepare a Ni-FeO catalyst. x / SiO2 catalyst, in which the mass fraction of Ni is 20.0% and the mass fraction of Fe is 5.0%, recorded as 20%Ni-5%FeO x / SiO2, the corresponding Fe / Ni ratio is 1 / 4.

[0084] The catalyst activity evaluation method provided in Example 1 is basically the same, but the evaluation conditions are different. When evaluating the catalytic activity of the catalyst prepared in Example 8, the volume space velocity includes 4 different values. The specific catalytic activity evaluation results are detailed in Table 6.

[0085] Table 6 20%Ni-5%FeO x Catalytic activity of SiO2 catalyst under different reaction conditions

[0086]

[0087]

[0088] It can be seen from Table 6 that when the reaction temperature, hydrogen pressure, HBPA / liquid ammonia molar ratio and H2 / HBPA molar ratio are the same, with the increase of volume space velocity, the conversion rate of hydrogenated bisphenol A gradually decreases, and the volume space velocity is between 0.1 and 0.3 h -1 When the conversion rate was between 2 and 3 , the conversion rate did not change substantially, while the selectivity of 2,2-bis(4-aminocyclohexyl)propane first increased and then decreased.

[0089] Embodiment 9-embodiment 10

[0090] Example 9 is the same as Example 1, except that when the catalyst is prepared by the ammonia evaporation method, the masses of the Ni salt and the Fe salt added are different. Specifically: Example 8 weighs 66.95 g of Ni(NO3)2·6H2O and 29.35 g of Fe(NO3)3·9H2O in a 1000 mL round-bottom flask to prepare a Ni-FeO catalyst. x / SiO2 catalyst, in which the mass fraction of Ni is 20.0% and the mass fraction of Fe is 6.0%, recorded as 20%Ni-6%FeO x / SiO2, the corresponding Fe / Ni ratio is 3 / 10.

[0091] Example 10 Weigh 63.52 g of Ni(NO3)2·6H2O and 9.27 g of Fe(NO3)3·9H2O in a 1000 mL round-bottom flask to prepare a Ni-FeO catalyst. x / SiO2 catalyst, in which the mass fraction of Ni is 20.0% and the mass fraction of Fe is 2.0%, recorded as 20%Ni-2%FeO x / SiO2, the corresponding Fe / Ni ratio is 1 / 10.

[0092] According to the catalyst activity evaluation method provided in Example 1, the catalytic activity of the catalysts prepared in Example 9 and Example 10 was evaluated. The catalytic activity evaluation results are shown in Table 7.

[0093] Table 7 Catalytic activity of catalysts with different promoter ratios

[0094]

[0095] Comparing the experimental results in Table 4, Table 6 and Table 7, it can be seen that as the Fe / Ni ratio increases, the catalyst activity increases, and when the Fe / Ni ratio is greater than 1 / 4, the selectivity of the catalytic reaction decreases.

[0096] Preferably, the Ni—FeO x The Fe / Ni ratio in / SiO2 catalyst is 1 / 10~1 / 4.

[0097] Example 11 to Example 12

[0098] Example 11 and Example 12 are the same as Example 8, except that the calcination temperature is different when the catalyst is prepared by the ammonia evaporation method. Since the mass fractions of the active components and additives in Example 8, Example 11 and Example 12 are the same, in order to distinguish the three, the temperature is added after the catalyst to distinguish them. Specifically, the catalyst prepared in Example 8 is represented by 20% Ni-5% FeO x / SiO2-600°C, the catalyst prepared in Example 11 is represented by 20%Ni-5%FeO x / SiO2-500°C, the catalyst prepared in Example 12 is represented by 20%Ni-5%FeO x / SiO2-800℃,

[0099] According to the catalyst activity evaluation method provided in Example 1, the catalytic activity of the catalysts prepared in Example 11 and Example 12 was evaluated. The catalytic activity evaluation results are shown in Table 8.

[0100] Table 8 Catalytic activity of catalysts prepared at different calcination temperatures

[0101]

[0102] It can be seen from Table 8 that when the calcination temperature of the catalyst increases to 800°C, the selectivity of the catalytic reaction decreases significantly. It may be that the high calcination temperature causes some active components in the catalyst to agglomerate.

[0103] Preferably, the calcination temperature is 500°C to 600°C.

[0104] Comparative Example 1

[0105] Weigh 66.06g of Ni(NO3)2·6H2O and 24.13g of Fe(NO3)3·9H2O and dissolve them in 200g of purified water, add 50g of SiO2 carrier, stir thoroughly, slowly add sodium carbonate solution until pH ≥ 8.5, filter, wash the filter cake with purified water until pH = 7, then dry it in an oven at 120℃ for 12h, and calcine the obtained catalyst at 600℃ in a muffle furnace for 6h to obtain Ni-FeO x @SiO2 catalyst, where the Ni loading is 20.0% and the Fe loading is 5.0%, recorded as 20%Ni-5%FeO x / SiO2-D.

[0106] According to the catalyst activity evaluation method provided in Example 1, the catalytic activity of the catalyst prepared in Comparative Example 1 was evaluated. The catalytic activity evaluation results are shown in Table 9.

[0107] Table 9 Ni-FeO prepared by different preparation methods x @Catalytic activity of SiO2 catalyst

[0108]

[0109] It can be seen from Table 9 that the catalyst prepared by the ammonia distillation method has higher selectivity and relatively higher conversion rate than the supported catalyst prepared in Comparative Example 1. The main reason is that the active component Ni in the catalyst has higher dispersion, higher activity and high primary amine selectivity.

[0110] Comparative Example 2

[0111] Comparative Example 2 is the same as Example 1, except that when the catalyst is prepared by the ammonia evaporation method, no auxiliary agent is added and the amount of Ni salt added is different. Specifically: In Comparative Example 2, only 61.93 g of Ni(NO3)2·6H2O is weighed into a 1000 mL round-bottom flask, and the prepared catalyst is a Ni / SiO2 catalyst, in which the mass fraction of Ni is 20.0%, recorded as 20% Ni / SiO2.

[0112] According to the catalyst activity evaluation method provided in Example 1, the catalytic activity of the catalyst prepared in Comparative Example 2 was evaluated. The catalytic activity evaluation results are shown in Table 10.

[0113] Table 10 Ni-FeO x Comparison of catalytic activity between @SiO2 catalyst and Ni / SiO2 catalyst

[0114]

[0115] It can be seen from Table 10 that the catalyst with the introduction of metal oxide has higher conversion rate and selectivity. On the one hand, the addition of Fe increases the adsorption capacity of the raw material, thereby increasing the dehydrogenation reaction rate of the alcohol. At the same time, the addition of Fe forms an alloy with Ni, isolates the metal site of Ni, inhibits the coupling reaction of amines, and improves the selectivity of primary amines. On the other hand, after the introduction of metal oxide, due to the synergistic effect of metal oxide / metal and Ni metal, the agglomeration of metal Ni and the coking of the catalyst surface are further inhibited, and the condensation side reaction is reduced, and the yield of the target product 2,2-bis-(4-aminocyclohexyl)propane is high.

[0116] Embodiment 11

[0117] Catalyst life evaluation

[0118] The catalyst 20% Ni-5% FeO prepared in Example 8 x / SiO2 and the catalyst prepared in Comparative Example 1 20%Ni-5%FeO x The stability of the catalyst prepared by / SiO2-D was tested.

[0119] The catalyst life evaluation was carried out according to the catalyst activity evaluation method provided in Example 1. The evaluation conditions were as follows: hydrogen pressure 10 MPa, HBPA / ammonia = 1 / 6, reaction temperature 220°C, volume space velocity 0.3 h -1 , H2 / HBPA molar ratio = 4 / 1.

[0120] The catalyst life evaluation results of the catalysts prepared in Example 8 and Comparative Example 1 are shown in Table 11.

[0121] Table 11 20%Ni-5%FeO x / SiO2 and 20%Ni-5%FeO x / SiO2-D stability comparison results

[0122]

[0123] It can be seen from Table 11 that the catalytic reaction yield of the catalyst prepared by the ammonia distillation method is significantly higher than that of the supported catalyst, and the stability of the catalyst is significantly enhanced.

[0124] It should be noted that the conversion rate in the above table refers to the conversion rate of hydrogenated bisphenol A, and the selectivity refers to the selectivity of 2,2-bis-(4-aminocyclohexyl)propane.

[0125] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions and substitutions can be made without departing from the concept of the present invention, which should be regarded as belonging to the protection scope of the present invention.

Claims

1. A method for preparing 2,2-bis(4-aminocyclohexyl)propane by hydrogenating bisphenol A, characterized in that: The method comprises: using a fixed bed reactor as a reaction site, and under a catalyst and preset reaction conditions, causing a hydrogenated bisphenol A solution, liquid ammonia and hydrogen to undergo a hydroamination reaction to prepare 2,2-bis(4-aminocyclohexyl)propane, wherein the catalyst is a Ni-B / SiO2 catalyst prepared by an ammonia evaporation method, and the preset reaction conditions include: a hydrogen pressure of 8MPa to 12MPa, a reaction temperature of 180 to 240°C, and a volume space velocity of 0.1h -1 ~0.6h -1 ; Wherein, the Ni-B / SiO2 catalyst includes an active component Ni, an additive B and a carrier SiO2, and a nickel sheet silicate structure is formed between the active component Ni and the carrier SiO2. Based on the total weight of the Ni-B / SiO2 catalyst as 100%, the mass percentage of the active component Ni is 10 to 25%.

2. The method for preparing 2,2-bis(4-aminocyclohexyl)propane by hydroamination of hydrogenated bisphenol A according to claim 1, characterized in that: The auxiliary agent B is an oxide of an auxiliary element, and the auxiliary element is selected from one or a combination of at least two of K, Na, Ce, Ca, Fe, La, Mg, and Ba. Based on the total weight of the catalyst as 100%, the mass percentage of the auxiliary element is 2-6%.

3. The method for preparing 2,2-bis(4-aminocyclohexyl)propane by hydroamination of hydrogenated bisphenol A according to claim 2, characterized in that: The ammonia evaporation method is specifically as follows: nickel nitrate and metal salts of auxiliary elements are first prepared into a solution, ammonia water is added dropwise for complexation, silica sol is added dropwise at 20-60° C., and the dropping time is controlled to be 0.5 h to 4 h. After the dropping is completed, the temperature is kept for 1 h to 4 h, and then the temperature is raised to 60-100° C. to evaporate ammonia until the mother liquor pH is 6, and the ammonia evaporation is stopped. The feed liquid after ammonia evaporation is filtered, washed, dried, and roasted to obtain the catalyst.

4. The method for preparing 2,2-bis(4-aminocyclohexyl)propane by hydroamination of hydrogenated bisphenol A according to claim 3, characterized in that: In the ammonia evaporation method, the drying temperature is 100-150° C. and the drying time is 6 h to 15 h.

5. The method for preparing 2,2-bis(4-aminocyclohexyl)propane by hydroamination of hydrogenated bisphenol A according to claim 3, characterized in that: In the ammonia distillation method, the roasting temperature is 500-800° C. and the roasting time is 2 h to 8 h.

6. The method for preparing 2,2-bis(4-aminocyclohexyl)propane by hydroamination of hydrogenated bisphenol A according to any one of claims 1 to 5, characterized in that: The method further comprises reducing the Ni-B / SiO2 catalyst before the hydroamination reaction, wherein the reduction of the Ni-B / SiO2 catalyst is specifically as follows: using a mixture of hydrogen and nitrogen as a reducing agent, the reduction temperature is 400-700° C., the reduction time is 2h-8h, wherein the volume percentage of hydrogen in the mixture of hydrogen and nitrogen is 10-90%, and the hydrogen volume space velocity is 50h -1 ~300h -1 .

7. The method for preparing 2,2-bis(4-aminocyclohexyl)propane by hydroamination of hydrogenated bisphenol A according to claim 1, characterized in that: The hydrogenated bisphenol A solution comprises hydrogenated bisphenol A and a solvent, wherein the solvent is one of dioxane, ethylene glycol dimethyl ether, ethylene glycol diethyl ether and tetrahydrofuran.

8. The method for preparing 2,2-bis(4-aminocyclohexyl)propane by hydroamination of hydrogenated bisphenol A according to claim 7, characterized in that: Based on the total weight of the hydrogenated bisphenol A solution being 100%, the mass fraction of the hydrogenated bisphenol A is 10-30wt%.

9. The method for preparing 2,2-bis(4-aminocyclohexyl)propane by hydroamination of hydrogenated bisphenol A according to claim 7, characterized in that: The molar ratio of the hydrogenated bisphenol A to liquid ammonia is 1:(4-10), and the molar ratio of the hydrogenated bisphenol A to H2 is 1:(2-6).

10. The method for preparing 2,2-bis(4-aminocyclohexyl)propane by hydroamination of hydrogenated bisphenol A according to claim 1, characterized in that: The reaction temperature is 220-240°C.

Citation Information

Patent Citations

  • Production of BIS-(4-aminocyclohexyl)-alkanes

    US3551485A