Water-borne epoxy resin as well as preparation method and application thereof

By reacting acid anhydride compounds with branched alcohol compounds to modify the epoxy resin and emulsifying under shear conditions, the problems of high viscosity and poor toughness of the aqueous epoxy resin are solved, and high epoxy equivalent and stability are improved. The coating performance is optimized for a variety of curing systems.

CN119019646APending Publication Date: 2024-11-26JIANGSU FUQISEN NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411292093.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The molecular weight of existing aqueous epoxy resins is relatively large, resulting in high viscosity, high coating hardness and poor toughness, making it difficult to use in amino resin or isocyanate curing systems. During the preparation process, there is a large amount of solvent, a high VOC content, and poor emulsion stability.

Method used

Carboxylic acid compound is formed by reacting an anhydride compound with branched alcohol compounds, and the carboxylic acid compound is carried out with an epoxy resin under a catalyst to obtain a modified epoxy resin, which is then blended with an emulsifier and a solvent and drops under shearing conditions Water emulsification was added to prepare an aqueous epoxy resin with a high epoxy equivalent and hydroxyl content.

Benefits of technology

Improve the toughness of aqueous epoxy resin, reduce viscosity and solvent usage, enhance the stability of the emulsion, and make it useful in a variety of curing systems. The coating has fast drying speed, significantly improved media corrosion resistance and flexibility, and the process Simple, easy to obtain raw materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019646A_ABST
    Figure CN119019646A_ABST
Patent Text Reader

Abstract

The invention provides waterborne epoxy resin as well as a preparation method and application thereof, and belongs to the technical field of coatings. The preparation method comprises the following steps: reacting an anhydride compound with a branched alcohol compound to obtain a carboxylic acid compound, and then carrying out ring-opening reaction on the carboxylic acid compound and epoxy resin under the action of a catalyst to obtain modified epoxy resin; and finally, blending the emulsifier, the modified epoxy resin and the solvent, and dropwise adding water for emulsification under shearing to obtain the water-borne epoxy resin. The epoxy resin is modified by the carboxyl compound synthesized by the branched alcohol compound, compared with dimer acid modified resin, the viscosity is smaller, the emulsification is easier to carry out, the stability of the obtained emulsion is higher, meanwhile, the water-borne epoxy resin prepared by the method can be cured in three curing modes, and the performance of an obtained coating film is better.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of coatings, and in particular to a waterborne epoxy resin and a preparation method and application thereof. Background Art

[0002] Epoxy resin is widely used in the field of coatings due to its excellent mechanical strength, corrosion resistance, excellent adhesion to metals and low volume shrinkage. Compared with solvent-based epoxy coatings, water-based epoxy coatings use water as a dispersion medium, which reduces pollution to the environment and improves the safety of coating use.

[0003] As a film former for waterborne epoxy coatings, waterborne epoxy resin has a huge impact on the performance of waterborne epoxy coatings. The waterborne epoxy resin on the market generally has a solid content of 53-60% and an epoxy equivalent of 800-1200 g / eq. The coating prepared using this resin already has excellent comprehensive performance, but there are still some conditions that need to be improved, such as the slow drying time of the coating due to the low epoxy equivalent; the poor flexibility of the coating due to the strong rigidity of the epoxy resin itself; and the low hydroxyl content in the resin makes it difficult to use in amino resin curing systems or isocyanate curing systems that require hydroxyl curing.

[0004] Most of the above conditions can be improved by increasing the epoxy equivalent of waterborne epoxy resin. Increasing the epoxy equivalent can increase the glass transition temperature and make it dry faster. At the same time, increasing the epoxy equivalent can increase the hydroxyl content in the waterborne epoxy resin, so that it can be used in amino resin curing systems and isocyanate curing systems. However, when the resin with high epoxy equivalent contains more polar groups such as hydroxyl groups, the molecular weight is large and the resin viscosity is large. It is necessary to add more solvents to reduce its viscosity, so that the resin VOC content is high and the solid content is low; at the same time, it will also cause the resin to be difficult to emulsify during emulsification, and the prepared waterborne epoxy resin is difficult to stabilize in water and is prone to sedimentation, resulting in poor emulsion stability. For example, in CN202010608158.2, a polyether compound and an epoxy resin are first used to prepare an emulsifier, and then diethanolamine is used, and the epoxy resin and the emulsifier react, and finally water is added for emulsification to obtain a waterborne epoxy resin. The epoxy resin used in the water-based epoxy resin prepared by the above method has a large molecular weight, so the coating film prepared by the water-based epoxy resin has a high hardness and poor toughness. At the same time, due to the large molecular weight of the epoxy resin used, its viscosity is large, and more solvents need to be added to reduce its viscosity. The prepared emulsion has a low solid content and a high VOC content.

[0005] Therefore, it is of great significance to provide a waterborne epoxy resin with a high solid content, which can improve the toughness of waterborne epoxy resin coatings, reduce the viscosity and overall solvent usage during the preparation of waterborne epoxy resins, and can be simultaneously applied to a variety of curing systems. Summary of the invention

[0006] The object of the present invention is to provide a water-based epoxy resin and a preparation method and application thereof, so as to solve the technical problems that the water-based epoxy resin in the prior art has a large molecular weight, resulting in a large viscosity, and the coating film prepared by the water-based epoxy resin has a high hardness and poor toughness, and is difficult to be used in an amino resin curing system or an isocyanate curing system.

[0007] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0008] The present invention provides a method for preparing a waterborne epoxy resin, comprising the following steps:

[0009] (1) reacting an acid anhydride compound with a branched alcohol compound to obtain a carboxylic acid compound;

[0010] (2) subjecting the carboxylic acid compound and the epoxy resin to a ring-opening reaction under the action of a catalyst to obtain a modified epoxy resin;

[0011] (3) The emulsifier, modified epoxy resin and solvent are mixed, and water is added dropwise under shearing to emulsify the mixture, thereby obtaining a water-based epoxy resin.

[0012] Further, the acid anhydride compound includes one or more of succinic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, nadic anhydride, methyl nadic anhydride, phthalic anhydride, methyl succinic anhydride, itaconic anhydride, maleic anhydride, methyl hexahydrophthalic anhydride, methyl tetrahydrophthalic anhydride, n-octyl succinic anhydride, n-dodecyl succinic anhydride and n-tetradecyl succinic anhydride;

[0013] The branched alcohol compound includes one or more of 2-butyl-2-ethyl-1,3-propanediol, 2-butyl-1,3-propanediol, 2-tert-butylpropane-1,3-diol, 2-methyl-2,4-pentanediol, neopentyl glycol, 2,5-dimethyl-2,5-hexanediol, 3,6-dimethyl-3,6-octanediol, 2-(2-hydroxypropane-2-yl)-5-methylcyclohexanol and 2-cyclohexylpropane-1,3-diol.

[0014] Furthermore, in the step (1), the molar ratio of the acid anhydride compound to the branched alcohol compound is 1 to 4:1;

[0015] The reaction temperature is 0-160° C., and the reaction time is 0.5-9 h.

[0016] Furthermore, in step (2), the epoxy resin is bisphenol A epoxy resin and / or bisphenol F epoxy resin; the epoxy equivalent of the epoxy resin is 100 to 500 g / eq;

[0017] The catalyst comprises one or more of N,N-dimethylbenzylamine, triphenylphosphine, boron trifluoride ethyl etherate, dibutyltin dilaurate, tributylamine and tetramethylammonium bromide.

[0018] Furthermore, the mass ratio of the carboxylic acid compound, the epoxy resin and the catalyst is 50-140:60-150:0.1-0.3;

[0019] The temperature of the ring-opening reaction is 80-160° C., and the time of the ring-opening reaction is 1-7 hours.

[0020] Furthermore, the emulsifier is obtained by reacting polyethylene glycol and epoxy resin in the presence of the catalyst described in step (2), wherein the mass ratio of polyethylene glycol, epoxy resin and catalyst is 50-180:60-190:0.1-0.3;

[0021] The solvent is one or more of acetone, butanone, methyl isobutyl ketone, ethylene glycol methyl ether, propylene glycol methyl ether, propylene glycol ethyl ether, propylene glycol butyl ether, dipropylene glycol methyl ether, dipropylene glycol ethyl ether, dipropylene glycol butyl ether, cyclohexane and benzyl alcohol.

[0022] Furthermore, the mass ratio of the modified epoxy resin, the emulsifier and the water is 160-240:20-30:120-180;

[0023] The mass ratio of the modified epoxy resin to the solvent is 160-240:40-60.

[0024] Furthermore, the shear rate is 1000-4000 r / min, the water drop acceleration rate is 1-20 mL / min, the emulsification temperature is 50-80° C., and the emulsification time is 20-40 min.

[0025] The invention provides a water-based epoxy resin prepared by the preparation method of the water-based epoxy resin.

[0026] The present invention also provides an application of a waterborne epoxy resin in a curing agent system, wherein the curing system comprises an epoxy curing agent curing system, an amino resin curing system or an isocyanate curing system.

[0027] Beneficial effects of the present invention:

[0028] (1) The waterborne epoxy resin prepared by the present invention has a hydroxyl content of about 3.0% and an epoxy equivalent weight of about 3100 g / eq, so that it can be used in epoxy curing agent curing system, amino resin curing system and isocyanate curing system;

[0029] (2) The present invention modifies the epoxy resin by using a carboxylic acid compound synthesized from an acid anhydride compound and a branched alcohol compound, thereby introducing a branched chain into the epoxy resin, reducing the viscosity of the modified resin, making the emulsification process easier, improving the stability of the emulsion, and reducing the use of solvents during emulsification;

[0030] (3) When the waterborne epoxy resin prepared by the present invention is added to a common epoxy resin, the drying speed of the waterborne epoxy resin coating can be increased due to the high molecular weight of the epoxy resin; at the same time, the large amount of flexible branched chains introduced increase the free volume between molecules and significantly improve the toughness of the coating;

[0031] (4) When the waterborne epoxy resin prepared by the present invention is added with a hydroxy acrylate dispersion and applied to an isocyanate curing system or an amino resin curing system, the medium corrosion resistance and flexibility can be improved;

[0032] (5) The preparation method of the present invention is simple and the raw materials are cheap and readily available. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is the infrared absorption spectrum of methylhexahydrophthalic anhydride, carboxylic acid compound B and modified epoxy resin in Example 2. DETAILED DESCRIPTION

[0034] The present invention provides a method for preparing a waterborne epoxy resin, comprising the following steps:

[0035] (1) reacting an acid anhydride compound with a branched alcohol compound to obtain a carboxylic acid compound;

[0036] (2) subjecting the carboxylic acid compound and the epoxy resin to a ring-opening reaction under the action of a catalyst to obtain a modified epoxy resin;

[0037] (3) The emulsifier, modified epoxy resin and solvent are mixed, and water is added dropwise under shearing to emulsify the mixture, thereby obtaining a water-based epoxy resin.

[0038] In the present invention, the acid anhydride compound includes one or more of succinic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, nadic anhydride, methyl nadic anhydride, phthalic anhydride, methyl succinic anhydride, itaconic anhydride, maleic anhydride, methyl hexahydrophthalic anhydride, methyl tetrahydrophthalic anhydride, n-octyl succinic anhydride, n-dodecyl succinic anhydride and n-tetradecyl succinic anhydride, preferably succinic anhydride, nadic anhydride, methyl nadic anhydride, phthalic anhydride, methyl succinic anhydride, One or more of dianhydride, itaconic anhydride, maleic anhydride, methylhexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, n-octylsuccinic anhydride, n-dodecylsuccinic anhydride and n-tetradecylsuccinic anhydride, and more preferably one or more of succinic anhydride, nadic anhydride, methylnadic anhydride, phthalic anhydride, itaconic anhydride, methylhexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, n-octylsuccinic anhydride, n-dodecylsuccinic anhydride and n-tetradecylsuccinic anhydride.

[0039] In the present invention, the branched alcohol compound includes one or more of 2-butyl-2-ethyl-1,3-propanediol, 2-butyl-1,3-propanediol, 2-tert-butylpropane-1,3-diol, 2-methyl-2,4-pentanediol, neopentyl glycol, 2,5-dimethyl-2,5-hexanediol, 3,6-dimethyl-3,6-octanediol, 2-(2-hydroxypropane-2-yl)-5-methylcyclohexanol and 2-cyclohexylpropane-1,3-diol, preferably 2-butyl-2-ethyl-1,3-propanediol, 2-butyl-1,3-propanediol, 2-methyl-2,4-pentanediol, neopentyl glycol, 2,5-dimethyl-2,5-hexanediol, 3,6-dimethyl-3,6-octanediol, 2-(2-hydroxypropane-2-yl)-5-methylcyclohexanol and 2-cyclohexylpropane-1,3-diol. One or more of alcohol, neopentyl glycol, 2,5-dimethyl-2,5-hexanediol, 3,6-dimethyl-3,6-octanediol, 2-(2-hydroxypropane-2-yl)-5-methylcyclohexanol and 2-cyclohexylpropane-1,3-diol, and more preferably one or more of 2-butyl-2-ethyl-1,3-propanediol, 2-methyl-2,4-pentanediol, neopentyl glycol, 2,5-dimethyl-2,5-hexanediol, 3,6-dimethyl-3,6-octanediol, 2-(2-hydroxypropane-2-yl)-5-methylcyclohexanol and 2-cyclohexylpropane-1,3-diol.

[0040] In the present invention, branched alcohol compounds are alcohol compounds with a branched structure, and the carbon chain in the molecule of this type of compound is not a completely straight chain, but contains at least one branch. The modified epoxy resin synthesized by the branched alcohol compound can reduce the intermolecular interaction force due to the branched structure with branched alcohol, improve the intermolecular free volume, reduce the synthetic resin viscosity, and simultaneously because the epoxy resin has a branched spatial structure and a flexible segment, the toughness of the resin can also be improved. Therefore, the branched alcohol compounds are introduced into the epoxy resin, which can solve the problem that the macromolecular epoxy resin is difficult to emulsify because of the high viscosity, and can solve the problem that a large amount of solvents need to be introduced in its emulsification process.

[0041] In the present invention, in the step (1), the molar ratio of the acid anhydride compound to the branched alcohol compound is 1 to 4:1, preferably 1.2 to 3.8:1, and more preferably 1.5 to 3.5:1.

[0042] In the present invention, the reaction temperature is 0 to 160° C., preferably 40 to 150° C., and more preferably 80 to 130° C.; the reaction time is 0.5 to 9 h, preferably 1 to 8 h, and more preferably 2 to 7 h.

[0043] In the present invention, in step (2), the epoxy resin is a bisphenol A epoxy resin and / or a bisphenol F epoxy resin, preferably a bisphenol A epoxy resin; the epoxy equivalent of the epoxy resin is 100 to 500 g / eq, preferably 150 to 500 g / eq, and more preferably 190 to 500 g / eq.

[0044] In the present invention, the catalyst comprises one or more of N,N-dimethylbenzylamine, triphenylphosphine, boron trifluoride ethyl ether, dibutyltin dilaurate, tributylamine and tetramethylammonium bromide, preferably one or more of N,N-dimethylbenzylamine, triphenylphosphine, dibutyltin dilaurate, tributylamine and tetramethylammonium bromide, and further preferably one or more of N,N-dimethylbenzylamine, triphenylphosphine, tributylamine and tetramethylammonium bromide.

[0045] In the present invention, the mass ratio of the carboxylic acid compound, the epoxy resin and the catalyst is 50-140:60-150:0.1-0.3, preferably 80-135:65-148.5:0.15-0.28, and more preferably 100-130:70-145:0.18-0.25.

[0046] In the present invention, the temperature of the ring-opening reaction is 80 to 160° C., preferably 85 to 155° C., and more preferably 90 to 150° C.; the time of the ring-opening reaction is 1 to 7 h, preferably 1.5 to 6 h, and more preferably 2 to 5 h.

[0047] In the present invention, the emulsifier is obtained by reacting polyethylene glycol and epoxy resin in the presence of the catalyst described in step (2), wherein the mass ratio of polyethylene glycol, epoxy resin and catalyst is 50-180:60-190:0.1-0.3, preferably 55-175:65-185:0.1-0.25, and more preferably 60-170:70-180:0.1-0.2.

[0048] In the present invention, the solvent is one or more of acetone, butanone, methyl isobutyl ketone, ethylene glycol methyl ether, propylene glycol methyl ether, propylene glycol ethyl ether, propylene glycol butyl ether, dipropylene glycol methyl ether, dipropylene glycol ethyl ether, dipropylene glycol butyl ether, cyclohexane and benzyl alcohol, preferably one or more of acetone, methyl isobutyl ketone, ethylene glycol methyl ether, propylene glycol methyl ether, propylene glycol ethyl ether, propylene glycol butyl ether, dipropylene glycol methyl ether, dipropylene glycol ethyl ether, dipropylene glycol butyl ether, cyclohexane and benzyl alcohol, further preferably one or more of acetone, methyl isobutyl ketone, ethylene glycol methyl ether, propylene glycol methyl ether, propylene glycol butyl ether, dipropylene glycol methyl ether, dipropylene glycol ethyl ether, dipropylene glycol butyl ether, cyclohexane and benzyl alcohol.

[0049] In the present invention, the mass ratio of the modified epoxy resin, the emulsifier and water is 160-240:20-30:120-180, preferably 165-235:21-29:122-176, and more preferably 170-232:22-28:124-174;

[0050] The mass ratio of the modified epoxy resin to the solvent is 160-240:40-60, preferably 165-235:42-58, and more preferably 170-232:44-56.

[0051] In the present invention, the shear rate is 1000-4000 r / min, preferably 1200-3800 r / min, and more preferably 1500-3500 r / min; the water drop acceleration rate is 1-20 mL / min, preferably 2-18 mL / min, and more preferably 3-15 mL / min; the emulsification temperature is 50-80°C, preferably 55-75°C, and more preferably 60-70°C; the emulsification time is 20-40 min, preferably 22-39 min, and more preferably 24-35 min.

[0052] The invention provides a water-based epoxy resin prepared by the preparation method of the water-based epoxy resin.

[0053] The present invention also provides an application of a waterborne epoxy resin in a curing agent system, wherein the curing system comprises an epoxy curing agent curing system, an amino resin curing system or an isocyanate curing system.

[0054] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0055] Example 1

[0056] 26.05 g of neopentyl glycol and 84.17 g of methyl hexahydrophthalic anhydride were reacted at 120° C. for 2 h to obtain a carboxylic acid compound A having a molecular weight of 440;

[0057] 110.22g of carboxylic acid compound A, 53.17g of epoxy resin E51 (epoxy equivalent is 190g / eq) and 53.17g of bisphenol F epoxy resin (epoxy equivalent is 175g / eq) are subjected to a ring-opening reaction under the action of 0.23g of tetramethylammonium bromide, the temperature of the ring-opening reaction is 125°C, the time of the ring-opening reaction is 2h, and after the reaction is completed, a modified epoxy resin is obtained;

[0058] 100g PEG6000, 65.27g epoxy resin E20 (epoxy equivalent is 500g / eq) and 0.16g triphenylphosphine are reacted at 125°C for 2h to obtain an emulsifier; 173.46g water (water dropping rate is 3mL / min) is added dropwise to 232.85g modified epoxy resin, 59.49g propylene glycol methyl ether and 30.15g emulsifier at a temperature of 60°C and a rotation speed of 3800r / min. After the addition is completed, the shear rate is adjusted to 2200r / min for emulsification for 35min to obtain a water-based epoxy resin.

[0059] Example 2

[0060] 34.69 g of 2-butyl-2-ethyl-1,3-propanediol and 72.8 g of methylhexahydrophthalic anhydride were reacted at 80° C. for 3 h to obtain a carboxylic acid compound B with a molecular weight of 496;

[0061] 124.9 g of carboxylic acid compound B and 125.1 g of epoxy resin E51 (epoxy equivalent is 190 g / eq) are subjected to a ring-opening reaction under the action of 0.22 g of triphenylphosphine, the temperature of the ring-opening reaction is 115° C., the time of the ring-opening reaction is 2 h, and after the reaction is completed, a modified epoxy resin is obtained;

[0062] 100g PEG6000, 65.27g epoxy resin E20 (epoxy equivalent is 500g / eq) and 0.16g triphenylphosphine are reacted at 125°C for 2h to obtain an emulsifier; 160g water (water dropping rate is 4mL / min) is added dropwise to 215g modified epoxy resin, 55.47g ethylene glycol butyl ether and 27.95g emulsifier at a temperature of 62°C and a rotation speed of 3000r / min. After the addition is completed, the shear rate is adjusted to 2100r / min for emulsification for 25min to obtain a water-based epoxy resin.

[0063] The methyl hexahydrophthalic anhydride, carboxylic acid compound B, and modified epoxy resin in Example 2 were subjected to infrared absorption spectrum test. The test results are as follows: Figure 1 As shown. Figure 1 It can be seen that the 1775 cm -1 The stretching vibration peak of the anhydride (C=O) disappeared, and at the same time, the peak at 3465 cm-1 There is no stretching vibration peak of -OH, 1732cm -1 The stretching vibration peak of carboxyl (C=O) appeared in the modified epoxy resin G, indicating that the carboxylic acid compound was successfully synthesized. -1 The stretching vibration of -OH appears, and at 916cm -1 The intensity of the epoxy bending vibration peak weakened, indicating that the modified epoxy resin was successfully synthesized.

[0064] Example 3

[0065] 34.69 g of 2-butyl-2-ethyl-1,3-propanediol and 72.8 g of methylhexahydrophthalic anhydride were reacted at 80° C. for 3 h to obtain a carboxylic acid compound B with a molecular weight of 496;

[0066] 100 g of carboxylic acid compound B, 89 g of epoxy resin E51 (epoxy equivalent of 190 g / eq) and 38.2 g of epoxy resin E20 (epoxy equivalent of 500 g / eq) were subjected to a ring-opening reaction under the action of 0.25 g of N,N-dimethylbenzylamine. The temperature of the ring-opening reaction was 120° C. The time of the ring-opening reaction was 3 h. After the reaction, a modified epoxy resin was obtained.

[0067] 100g PEG4000, 28.58g epoxy resin E44 (epoxy equivalent is 227g / eq) and 0.14g triphenylphosphine are reacted at 135°C for 2h to obtain an emulsifier; 148.4g water (water dropping rate is 3mL / min) is added dropwise to 200g modified epoxy resin, 50.88g methyl isobutyl ketone and 24.72g emulsifier at a temperature of 63°C and a rotation speed of 3500r / min. After the addition is completed, the shear rate is adjusted to 2600r / min for emulsification for 20min to obtain a water-based epoxy resin.

[0068] Example 4

[0069] 26.05 g of neopentyl glycol and 84.17 g of methyl hexahydrophthalic anhydride were reacted at 120° C. for 2 h to obtain a carboxylic acid compound A with a molecular weight of 440; 34.69 g of 2-butyl-2-ethyl-1,3-propanediol and 72.8 g of methyl hexahydrophthalic anhydride were reacted at 80° C. for 3 h to obtain a carboxylic acid compound B with a molecular weight of 496;

[0070] 40.86 g of carboxylic acid compound A, 81.72 g of carboxylic acid compound B and 127.4 g of epoxy resin E51 (epoxy equivalent is 190 g / eq) are subjected to a ring-opening reaction under the action of 0.19 g of tetramethylammonium bromide. The temperature of the ring-opening reaction is 130° C. The time of the ring-opening reaction is 3 h. After the reaction is completed, a modified epoxy resin is obtained;

[0071] 100g PEG4000, 28.58g epoxy resin E44 (epoxy equivalent is 227g / eq) and 0.14g triphenylphosphine are reacted at 135°C for 2h to obtain an emulsifier; 151.8g water (water dropping rate is 2mL / min) is added dropwise to 200g modified epoxy resin, 46.37g propylene glycol methyl ether and 23.46g emulsifier at a temperature of 67°C and a rotation speed of 2800r / min. After the addition is completed, the shear rate is adjusted to 2300r / min and emulsified for 28min to obtain a water-based epoxy resin.

[0072] Example 5

[0073] 16 g of 2-butyl-2-ethyl-1,3-propanediol and 42.4 g of n-octylsuccinic anhydride were reacted at 125° C. for 2 h to obtain a carboxylic acid compound C having a molecular weight of 584;

[0074] 133.63 g of carboxylic acid compound C and 116.37 g of epoxy resin E51 (epoxy equivalent is 190 g / eq) are subjected to a ring-opening reaction under the action of 0.18 g of triphenylphosphine. The temperature of the ring-opening reaction is 125° C. The time of the ring-opening reaction is 3 h. After the reaction is completed, a modified epoxy resin is obtained;

[0075] 100g PEG6000, 65.27g epoxy resin E20 (epoxy equivalent is 500g / eq) and 0.16g triphenylphosphine are reacted at 125°C for 2h to obtain an emulsifier; 155.83g water (water dropping rate is 3mL / min) is added dropwise to 210g modified epoxy resin, 53.42g ethylene glycol butyl ether and 25.96g emulsifier at a temperature of 66°C and a rotation speed of 3000r / min. After the addition is completed, the shear rate is adjusted to 2400r / min for emulsification for 29min to obtain a water-based epoxy resin.

[0076] Example 6

[0077] 34.69 g of 2-butyl-2-ethyl-1,3-propanediol and 72.8 g of methyl hexahydrophthalic anhydride were reacted at 80° C. for 3 h to obtain a carboxylic acid compound B with a molecular weight of 496; 13.4 g of 2,2-dihydroxymethylpropionic acid and 35.6 g of methyl nadic anhydride were reacted at 130° C. for 3 h to obtain a carboxylic acid compound D with a molecular weight of 490;

[0078] 109.89 g of carboxylic acid compound B, 12.21 g of carboxylic acid compound D and 128 g of epoxy resin E51 (epoxy equivalent is 190 g / eq) are subjected to a ring-opening reaction under the action of 0.23 g of tetramethylammonium bromide. The temperature of the ring-opening reaction is 125° C. The time of the ring-opening reaction is 2 h. After the reaction is completed, a modified epoxy resin is obtained;

[0079] 100g PEG4000, 28.58g epoxy resin E44 (epoxy equivalent is 227g / eq) and 0.14g triphenylphosphine are reacted at 135°C for 2h to obtain an emulsifier; 169.82g water (water dropping rate is 2mL / min) is added dropwise to 220g modified epoxy resin, 51.88g methyl isobutyl ketone and 30g emulsifier at a temperature of 65°C and a rotation speed of 3200r / min. After the addition is completed, the shear rate is adjusted to 2300r / min and emulsified for 27min to obtain a water-based epoxy resin.

[0080] Example 7

[0081] 16 g of 2-butyl-2-ethyl-1,3-propanediol and 42.4 g of n-octylsuccinic anhydride were reacted at 125° C. for 2 h to obtain a carboxylic acid compound C having a molecular weight of 584;

[0082] 50g of carboxylic acid compound C and 148.51g of epoxy resin E20 (epoxy equivalent is 500g / eq) are subjected to a ring-opening reaction under the action of 0.18g of triphenylphosphine, the temperature of the ring-opening reaction is 125°C, the time of the ring-opening reaction is 3h, and after the reaction is completed, a modified epoxy resin is obtained;

[0083] 100g PEG6000, 65.27g epoxy resin E20 (epoxy equivalent is 500g / eq) and 0.16g triphenylphosphine are reacted at 125°C for 2h to obtain an emulsifier; 124.66g water (water dropping rate is 3mL / min) is added dropwise to 168g modified epoxy resin, 42.74g ethylene glycol butyl ether and 20.77g emulsifier at a temperature of 66°C and a rotation speed of 3000r / min. After the addition is completed, the shear rate is adjusted to 2900r / min for emulsification for 24min to obtain a water-based epoxy resin.

[0084] Comparative Example 1

[0085] 100 g of dimer acid and 90.34 g of epoxy resin E51 (epoxy equivalent is 190 g / eq) were subjected to a ring-opening reaction under the action of 0.18 g of triphenylphosphine. The temperature of the ring-opening reaction was 125° C. The time of the ring-opening reaction was 3 h. After the reaction was completed, a modified epoxy resin was obtained.

[0086] 100 g of PEG6000, 65.27 g of epoxy resin E20 (epoxy equivalent weight: 500 g / eq) and 0.16 g of triphenylphosphine were reacted at 125° C. for 2 h to obtain an emulsifier;

[0087] 137.63 g of water was added dropwise to 184.8 g of modified epoxy resin, 46.52 g of ethylene glycol butyl ether and 22.85 g of emulsifier at a temperature of 66°C and a rotation speed of 3000 r / min (the water dropping rate was 3 mL / min). After the addition was completed, the shear rate was adjusted to 2500 r / min and emulsified for 20 minutes to obtain a water-based epoxy resin.

[0088] The performance of the waterborne epoxy resins prepared in Examples 1 to 7 and Comparative Example 1 was tested. The waterborne epoxy resin prepared in Comparative Example 1 was difficult to emulsify due to the high viscosity of the synthesized resin, and the obtained emulsion had a large particle size and poor storage stability, and precipitated after being stored at room temperature for two days. The test results of Examples 1 to 7 are shown in Table 1.

[0089] Table 1 Performance test results of waterborne epoxy resin prepared in Examples 1 to 7

[0090]

[0091]

[0092] The waterborne epoxy resin prepared in Examples 1 to 7 was applied to the amino resin curing system, and the specific steps were as follows: 55% of the waterborne epoxy resin prepared in Examples 1 to 7, 10% of 325 amino resin, 3% of ethylene glycol butyl ether, 3% of dipropylene glycol monomethyl ether, 0.3% of wetting agent Tego-270, 0.3% of wetting agent Tego-4100, 0.3% of leveling agent BYK-381, 0.2% of defoaming agent Tego-830, 0.4% of thickener 105A and 27.5% of white slurry R706 were mixed and sprayed on a polished iron plate to prepare a paint film, and then the paint film was cured at 80°C for 10 minutes after standing for leveling for 10 minutes, and finally cured at 140°C for 20 minutes, and then stood for 24 hours after the curing was completed. The properties of the prepared paint film were tested, and the test results are shown in Table 2. Among them, the viscosity is measured by a rotational viscometer, and the measurement standard is GB / T9751-1988; the particle size is measured in accordance with GBT19077-2016; the adhesion is measured by the cross-cut method, and the test standard is GB / T9286-1998; the pencil hardness of the paint film is measured in accordance with GB / T6739-1996; the flexibility of the paint film is measured in accordance with GB / T1731-1993; the 40°C water resistance is measured in accordance with GB / T5209-1985; the gloss is measured in accordance with GB / T13891-2009, and the gloss in the table refers to the gloss at 20° and 60°; the surface drying time is measured in accordance with GB / T1728-89; the impact is measured in accordance with GB / T1732-2020, and the table refers to a 50cm positive impact; the neutral salt spray resistance is measured in accordance with GB / T1771-2007.

[0093] Table 2 Performance of waterborne epoxy resins prepared in Examples 1 to 7 for use in amino resin curing systems

[0094] Test items Adhesion hardness Gloss / ° Flexibility / mm Impact / cm Resistant to normal temperature water Example 1 Level 0 2H 93 / 99 2 >50 >30d Example 2 Level 0 2H 95 / 100 1 >50 >30d Example 3 Level 0 3H 93.4 / 99 2 >50 >30d Example 4 Level 0 2H 95 / 100 1 >50 >30d Example 5 Level 0 2H 94 / 100 1 >50 >30d Example 6 Level 0 3H 92 / 99 2 >50 >30d Example 7 Level 0 4H 89 / 94 3 40 >30d

[0095] It can be seen from Table 1 and Table 2 that the waterborne epoxy resin prepared by the present invention has a higher solid content and a lower viscosity, and has good resistance to water at room temperature. The performance of the epoxy resin applied to the amino resin curing system meets the national standards and can meet the requirements of the baking varnish resin on the market.

[0096] The waterborne epoxy resin prepared in Examples 1 to 7 and AQUER-3011 epoxy emulsion (Jiangsu Fuqisen) were applied to the epoxy curing agent curing system, and the specific steps were as follows: 20% of the waterborne epoxy resin prepared in Examples 1 to 7, 20% of AQUER3011, 56.6% of pigment and filler slurry, 2.2% of cosolvent propylene glycol methyl ether, 0.3% of defoamer Tego-830, 0.5% of substrate wetting agent Tego-270, 0.2% of leveling agent BYK-381 and 0.2% of thixotropic additive XS83 were mixed and dispersed at high speed 20 to 30 minutes, component A of waterborne epoxy coating was obtained; propylene glycol methyl ether, water and AQUAC-3126 epoxy curing agent (Jiangsu Fuqisen) in a mass ratio of 1.5:1.5:7 were mixed to obtain component B; finally, component A and component B were formulated into coating according to a molar ratio of epoxy to amine hydrogen of 1:0.8, and then sprayed on polished tinplate and cold-rolled steel plate to prepare paint film. After the construction, the paint film was left to level for 30 minutes and then placed in an oven at 80°C for curing for 2 hours. After 24 hours, the performance test was carried out. The test results are shown in Table 3.

[0097] Table 3 Performance of waterborne epoxy resins prepared in Examples 1 to 7 applied to epoxy curing agent curing system

[0098]

[0099] As shown in Table 3, the waterborne epoxy resin prepared in the present invention has a higher epoxy equivalent, which shortens the surface drying time of the coating film, improves the neutral salt spray resistance, and improves the flexibility.

[0100] The waterborne epoxy resin prepared in Examples 1 to 7 was applied to an isocyanate curing system, and the specific steps were as follows: 30% of the waterborne epoxy resin prepared in Examples 1 to 7, 30% of AQUAPAC-8533, 29.5% of white paste R706, 3% of diethylene glycol butyl ether, 3% of dipropylene glycol monomethyl ether, 3% of propylene glycol methyl ether, 0.3% of wetting agent Tego-270, 0.3% of wetting agent Tego-4100, 0.5% of leveling agent BYK-381, 0.2% of defoaming agent Tego-830 and 0.2% of The thixotropic agent XS83 was mixed to obtain component A; 20% propylene glycol diacetate and 80% AQUAPU-298 isocyanate curing agent (Jiangsu Fuqisen) were mixed to obtain component B; component A and component B were mixed at a molar ratio of -NCO to -OH of 1.4:1 to prepare a coating, which was then sprayed on a polished tinplate and a cold-rolled steel plate to prepare a paint film. The paint film after construction was left to level for 30 minutes and then placed in a 70°C oven for curing for 2 hours. After being placed for 24 hours, the performance test was carried out. The test results are shown in Table 4.

[0101] Table 4 Performance of waterborne epoxy resins prepared in Examples 1 to 7 for use in isocyanate curing systems

[0102]

[0103] It can be seen from Table 4 that the waterborne epoxy resin prepared by the present invention has higher gloss and better resistance when cured in an isocyanate curing system, which can meet market requirements.

[0104] As can be seen from the above embodiments, the present invention provides a water-based epoxy resin and a preparation method and application thereof, wherein an acid anhydride compound and a branched alcohol compound are reacted to obtain a carboxylic acid compound, and then the carboxylic acid compound and the epoxy resin are subjected to a ring-opening reaction under the action of a catalyst to obtain a modified epoxy resin; finally, an emulsifier, a modified epoxy resin and a solvent are blended, and water is added dropwise under shearing to emulsify to obtain a water-based epoxy resin. The present invention uses a carboxyl compound synthesized from a branched alcohol compound to modify the epoxy resin, which has a lower viscosity than the dimer acid-modified resin, is easier to emulsify, and has a higher stability of the obtained emulsion. At the same time, the water-based epoxy resin prepared by the present invention can be cured by three curing methods, and the obtained coating performance is better.

[0105] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a waterborne epoxy resin, characterized in that: The following steps are involved: (1) reacting an acid anhydride compound with a branched alcohol compound to obtain a carboxylic acid compound; (2) subjecting the carboxylic acid compound and the epoxy resin to a ring-opening reaction under the action of a catalyst to obtain a modified epoxy resin; (3) The emulsifier, modified epoxy resin and solvent are mixed, and water is added dropwise under shearing to emulsify the mixture, thereby obtaining a water-based epoxy resin.

2. The method for preparing a waterborne epoxy resin according to claim 1, characterized in that: The acid anhydride compound includes one or more of succinic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, nadic anhydride, methyl nadic anhydride, phthalic anhydride, methyl succinic anhydride, itaconic anhydride, maleic anhydride, methyl hexahydrophthalic anhydride, methyl tetrahydrophthalic anhydride, n-octyl succinic anhydride, n-dodecyl succinic anhydride and n-tetradecyl succinic anhydride; The branched alcohol compound includes one or more of 2-butyl-2-ethyl-1,3-propanediol, 2-butyl-1,3-propanediol, 2-tert-butylpropane-1,3-diol, 2-methyl-2,4-pentanediol, neopentyl glycol, 2,5-dimethyl-2,5-hexanediol, 3,6-dimethyl-3,6-octanediol, 2-(2-hydroxypropane-2-yl)-5-methylcyclohexanol and 2-cyclohexylpropane-1,3-diol.

3. The method for preparing a waterborne epoxy resin according to claim 1 or 2, characterized in that: In the step (1), the molar ratio of the acid anhydride compound to the branched alcohol compound is 1 to 4:1; The reaction temperature is 0-160° C., and the reaction time is 0.5-9 h.

4. The method for preparing a waterborne epoxy resin according to claim 3, characterized in that: In the step (2), the epoxy resin is a bisphenol A epoxy resin and / or a bisphenol F epoxy resin; the epoxy equivalent of the epoxy resin is 100 to 500 g / eq; The catalyst comprises one or more of N,N-dimethylbenzylamine, triphenylphosphine, boron trifluoride ethyl etherate, dibutyltin dilaurate, tributylamine and tetramethylammonium bromide.

5. The method for preparing a waterborne epoxy resin according to claim 4, characterized in that: The mass ratio of the carboxylic acid compound, the epoxy resin and the catalyst is 50-140:60-150:0.1-0.3; The temperature of the ring-opening reaction is 80-160° C., and the time of the ring-opening reaction is 1-7 hours.

6. The method for preparing a waterborne epoxy resin according to claim 1, 2, 4 or 5, characterized in that: The emulsifier is obtained by reacting polyethylene glycol and epoxy resin in the presence of the catalyst described in step (2), wherein the mass ratio of polyethylene glycol, epoxy resin and catalyst is 50-180:60-190:0.1-0.3; The solvent is one or more of acetone, butanone, methyl isobutyl ketone, ethylene glycol methyl ether, propylene glycol methyl ether, propylene glycol ethyl ether, propylene glycol butyl ether, dipropylene glycol methyl ether, dipropylene glycol ethyl ether, dipropylene glycol butyl ether, cyclohexane and benzyl alcohol.

7. The method for preparing a waterborne epoxy resin according to claim 6, characterized in that: The mass ratio of the modified epoxy resin, the emulsifier and the water is 160-240:20-30:120-180; The mass ratio of the modified epoxy resin to the solvent is 160-240:40-60.

8. The method for preparing a waterborne epoxy resin according to claim 7, characterized in that: The shear rate is 1000-4000 r / min, the water drop acceleration rate is 1-20 mL / min, the emulsification temperature is 50-80° C., and the emulsification time is 20-40 min.

9. A water-based epoxy resin prepared by the method for preparing a water-based epoxy resin according to any one of claims 1 to 8.

10. Use of the waterborne epoxy resin according to claim 9 in a curing agent system, characterized in that: The curing system comprises an epoxy curing agent curing system, an amino resin curing system or an isocyanate curing system.