Preparation method and application of conductive hydrogel with environment resistance and freezing resistance

By introducing specific materials into the hydrogel to form multiple hydrogen bonds and physical crosslinks, the problem of insufficient anti-freeze and conductive properties of the hydrogel in extreme environments is solved, and the environmental and freezing resistance of conductive water is achieved Gel preparation, suitable for monitoring physiological signal in different extreme environments.

CN119019713APending Publication Date: 2024-11-26JILIN INST OF CHEM TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411285044.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing hydrogels have weak anti-freeze properties, poor anti-swelling properties, and insufficient conductivity in extreme environments, which limits their widespread use in wearable sensor applications.

Method used

Using poly(3,4-ethylenedioxythiophene)-polystyrene sulfonate, ethylene glycol, chitosan, acrylic acid, hydroxyethyl 2-methacrylate and ammonium persulfate aqueous solution, multiple levels are formed. Hydrogen bonding and physical cross-linking improve the mechanical properties and conductivity of the hydrogel, and prepare conductive hydrogels with environmental resistance and frost resistance.

Benefits of technology

The frost resistance, mechanical properties and electrical conductivity of the hydrogel are significantly improved, the swelling rate is reduced to -1.008%, the strain rate reaches 848.61%, and good application performance is maintained in different extreme environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019713A_ABST
    Figure CN119019713A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of flexible wearable sensor hydrogel, and particularly relates to a preparation method and application of conductive hydrogel with environment resistance and freezing resistance. Chitosan is introduced as a first network, acrylic acid and 2-hydroxyethyl methylacrylate are taken as monomers, deionized water and ethylene glycol are taken as binary solvents, poly (3, 4-ethylenedioxythiophene)-polystyrene sulfonate is taken as a conductive substance, an ammonium persulfate aqueous solution is taken as an initiator, and tannic acid is taken as a cross-linking agent, so that a second network is formed; the obtained hydrogel with environmental resistance, freezing resistance and conductivity has good environmental resistance (the swelling rate is-1.008%) and mechanical properties (the strain is 848.61% and the stress is 176.25 kPa), and the problem that existing hydrogel cannot give consideration to environmental resistance, freezing resistance and conductivity is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of flexible wearable sensor hydrogels, and in particular relates to a preparation method and application of a conductive hydrogel with environmental resistance and antifreeze properties. Background Art

[0002] Wearable hydrogel sensors have great development prospects in the hydrogel industry, especially in the fields of electronic skin and human health monitoring. However, traditional hydrogels have disadvantages such as poor anti-swelling performance, low tensile properties, and cannot be used in extreme environments. Therefore, the preparation of hydrogels with good tensile properties and can be used in extreme environments has attracted much attention in sensor applications.

[0003] The preparation of flexible wearable sensor hydrogels can solve the adverse effects of traditional wearable sensors such as poor mechanical properties, high swelling rate and weak conductivity. Due to the advantages of traditional hydrogels such as stretchability, flexibility and biocompatibility, they have become one of the candidate materials for wearable electronic devices and flexible strain sensors. However, due to their own hydrophilicity, traditional hydrogels will inevitably swell in aqueous environments. The swelling behavior will not only weaken the mechanical properties of the hydrogel, but also the expansion and collapse of the internal structure of the hydrogel system, which will damage the application performance of the flexible strain sensor. At present, the mechanical properties, anti-swelling properties and conductive properties of hydrogels are improved by constructing double network structures and enhancing cross-linking density. However, hydrogels still have defects such as weak antifreeze performance, poor anti-swelling performance and poor sensing performance, which greatly limit their application. Summary of the invention

[0004] The purpose of the present invention is to solve the problem that the existing hydrogel cannot take into account the environmental resistance, frost resistance and electrical conductivity. The present invention proposes a preparation method and application of a conductive hydrogel with environmental resistance and frost resistance.

[0005] The method for preparing a conductive hydrogel having environmental resistance and antifreeze properties comprises the following specific steps:

[0006] (1) adding poly(3,4-ethylenedioxythiophene)-polystyrene sulfonate into deionized water and stirring to obtain a mixed solution I;

[0007] (2) adding ethylene glycol to the mixed solution I, and stirring at 50° C. to obtain a mixed solution II;

[0008] (3) adding chitosan, acrylic acid, and 2-hydroxyethyl methacrylate monomer to the mixed solution II, stirring for 20-40 min at 50° C. until completely dissolved, to obtain a mixed solution III;

[0009] (4) After cooling the mixed solution III, an aqueous ammonium persulfate solution and tannic acid are added, and the mixture is stirred for 20-40 minutes until the mixture is completely dissolved to obtain a mixed solution IV; during this process, the mixture is cooled to room temperature, and then the aqueous ammonium persulfate solution and tannic acid are added to avoid the formation of flocs.

[0010] (5) Free radical polymerization of the mixed solution IV at 65° C. for 3-5 h to obtain a conductive hydrogel with environmental resistance and antifreeze properties.

[0011] In the present invention, deionized water: poly (3.4-ethylenedioxythiophene) - polystyrene sulfonate: ethylene glycol: chitosan: acrylic acid: 2-hydroxyethyl methacrylate: ammonium persulfate aqueous solution: tannic acid = (7-9) ml: (0.3-1.0) ml: (1-3) ml: (0.1-0.3) g: (1-5) ml: (3-5) ml: 1 ml: 0.005 g.

[0012] Preferably, deionized water: poly(3.4-ethylenedioxythiophene)-polystyrene sulfonate: ethylene glycol: chitosan: acrylic acid: 2-hydroxyethyl methacrylate: aqueous ammonium persulfate solution: tannic acid = 7 ml: 0.4 ml: 3 ml: 0.1 g: 2 ml: 5 ml: 1 ml: 0.005 g.

[0013] The concentration of the ammonium persulfate aqueous solution is 60 mg / mL.

[0014] In the present invention, chitosan is used as the first network; acrylic acid and 2-hydroxyethyl methacrylate are monomers, deionized water, ethylene glycol are binary solvents, poly(3,4-ethylenedioxythiophene)-polystyrene sulfonate is a conductive substance, an aqueous ammonium persulfate solution is used as an initiator, and tannic acid is used as a cross-linking agent to form a second network. Physical crosslinks with multiple hydrogen bonds are formed between the first network and the second network to enhance the mechanical properties of the hydrogel. Chitosan has hydrophilic amino and hydroxyl groups, acrylic acid contains hydrophilic carboxyl groups, and 2-hydroxyethyl methacrylate contains hydrophobic ester groups. The synergistic effect of hydrophilic and hydrophobic groups gives the hydrogel good environmental resistance. Ethylene glycol forms multiple hydrogen bonds with water molecules, which can effectively reduce the crystallization point of water molecules, thereby giving the hydrogel good antifreeze properties and improving the mechanical properties of the hydrogel. Because poly(3,4-ethylenedioxythiophene)-polystyrene sulfonate contains a large number of anions and cations, the prepared hydrogel has conductive properties. The electrostatic interaction formed by polystyrene sulfonate in the system can effectively inhibit the leakage of conductive substances in different water environments, thus making it have good conductive properties. Tannic acid, as a cross-linking agent, contains a large number of o-diphenol groups, which can provide a large number of cross-linking points, making the network structure more compact, and further enhancing its mechanical properties and environmental resistance.

[0015] The present invention has the following beneficial effects:

[0016] 1) The present invention introduces chitosan as the first network, acrylic acid and 2-hydroxyethyl methacrylate as monomers; deionized water and ethylene glycol as binary solvents, poly (3,4-ethylenedioxythiophene) -polystyrene sulfonate as a conductive substance, an aqueous solution of ammonium persulfate as an initiator, and tannic acid as a cross-linking agent to form a second network, thereby obtaining a hydrogel with environmental resistance, antifreeze and electrical conductivity, and having good environmental resistance (swelling rate -1.008%) and mechanical properties (strain: 848.61% and stress 176.25 kPa).

[0017] 2) The hydrogel prepared by the present invention has good antifreeze properties due to the action of multiple hydrogen bonds between ethylene glycol and water molecules.

[0018] 3) The hydrogel prepared by the present invention has environmental resistance, antifreeze and electrical conductivity, and has good electrical conductivity in the presence of poly(3,4-ethylenedioxythiophene)-polystyrene sulfonate.

[0019] 4) The hydrogel sensor prepared by the present invention has environmental resistance, antifreeze and electrical conductivity and can be used to monitor physiological signals in different extreme environments. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 The swelling curves of the hydrogels prepared in Example 1 and Comparative Example 1;

[0021] Figure 2 The swelling curves of the hydrogels prepared in Example 1 and Example 2;

[0022] Figure 3 The swelling curves of the hydrogels prepared in Example 1 and Example 3;

[0023] Figure 4 The swelling curves of the hydrogels prepared in Example 1 and Example 4;

[0024] Figure 5 1 is a swelling curve diagram of the hydrogels prepared in Example 1 and Example 5;

[0025] Figure 6 The swelling curves of the hydrogel prepared in Example 1 under different environments;

[0026] Figure 7 Graphs showing tensile stress-strain curves of the hydrogels prepared in Example 1 and Comparative Example 2;

[0027] Figure 8 The tensile stress-strain curves of the hydrogel prepared in Example 1 under different temperature environments;

[0028] Fig. 9The tensile stress-strain curves of the hydrogel prepared in Example 1 after being immersed in different aqueous environments;

[0029] Fig.10 The hydrogel prepared in Example 1 is used as a flexible wearable sensor to monitor human motion signals in an underwater environment. DETAILED DESCRIPTION

[0030] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0031] The experimental methods used in the following examples are conventional methods unless otherwise specified. The materials, reagents, methods and instruments used are conventional materials, reagents, methods and instruments in the art unless otherwise specified, and can be obtained through commercial channels by those skilled in the art.

[0032] The terms "comprising," "including," "having," "containing," or any other variations thereof, as used in the following examples, are intended to cover a non-exclusive inclusion. For example, a composition, step, method, article, or apparatus comprising the listed elements is not necessarily limited to only those elements, but may include other elements not expressly listed or inherent to such composition, step, method, article, or apparatus.

[0033] When equivalent, concentration or other value or parameter is represented by the range limited by range, preferred range or a series of upper preferred value and lower preferred value, this should be understood as specifically disclosing all ranges formed by any pairing of any upper range limit or preferred value and any lower range limit or preferred value, regardless of whether the scope is disclosed separately. For example, when disclosing range "1 to 5", described range should be interpreted as including range "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5" etc. When numerical range is described in this article, unless otherwise stated, the scope is intended to include its end value and all integers and fractions within the scope. In the present application specification and claims, range limitation can be combined and / or interchanged, if these ranges are not otherwise stated, include all sub-ranges contained therein.

[0034] The indefinite articles "a" and "an" before the elements or components of the present invention have no limitation on the quantity requirements (i.e. the number of occurrences) of the elements or components. Therefore, "a" or "an" should be interpreted as including one or at least one, and the elements or components in the singular form also include the plural form, unless the quantity obviously refers to the singular form only.

[0035] Example 1

[0036] The preparation of the hydrogel with environmental resistance, antifreeze properties and electrical conductivity of this embodiment is carried out according to the following steps:

[0037] Step 1: First, 7 mL of deionized water was added to a beaker, and then 0.4 mL of poly(3,4-ethylenedioxythiophene)-polystyrene sulfonate was added to the deionized water and stirred sufficiently to obtain a mixed solution I;

[0038] Step 2: Add 3 mL of ethylene glycol to the mixed solution I, and stir at 50° C. to obtain a mixed solution II;

[0039] Step 3: Add 0.1 g chitosan, 2 mL acrylic acid, and 5 mL 2-hydroxyethyl methacrylate monomer to the mixed solution II and stir thoroughly for 30 min at 50° C. until completely dissolved to obtain a mixed solution III;

[0040] Step 4: After the mixed solution III is cooled to 25°C, 1 mL of ammonium persulfate and 0.005 g of tannic acid are added, and stirred for 30 min until completely dissolved to obtain a mixed solution IV;

[0041] Step 5: Finally, the mixed solution IV is poured into a mold and free radical polymerized at 65°C for 4 hours to obtain a conductive hydrogel with environmental resistance and antifreeze properties.

[0042] Example 2

[0043] The preparation method of the hydrogel having environmental resistance, antifreeze property and electrical conductivity of the present embodiment is carried out by the following steps:

[0044] Step 1: First, 7 mL of deionized water was added to a beaker, and then 0.4 mL of poly(3,4-ethylenedioxythiophene)-polystyrene sulfonate was added to the deionized water and stirred sufficiently to obtain a mixed solution I;

[0045] Step 2: Add 3 mL of ethylene glycol to the mixed solution I, and stir at 50° C. to obtain a mixed solution II;

[0046] Step 3: Add 0.1 g chitosan, 5 mL acrylic acid, and 5 mL 2-hydroxyethyl methacrylate monomer to the mixed solution II and stir thoroughly for 30 min at 50° C. until completely dissolved to obtain a mixed solution III;

[0047] Step 4: After the mixed solution III is cooled to 25°C, 1 mL of ammonium persulfate and 0.005 g of tannic acid are added, and stirred for 30 min until completely dissolved to obtain a mixed solution IV;

[0048] Step 5: Finally, the mixed solution IV is poured into a mold and free radical polymerized at 65°C for 4 hours to obtain a conductive hydrogel with environmental resistance and antifreeze properties.

[0049] Example 3

[0050] The preparation of the hydrogel with environmental resistance, antifreeze properties and electrical conductivity of this embodiment is carried out according to the following steps:

[0051] Step 1: First, 7 mL of deionized water was added to a beaker, and then 0.4 mL of poly(3,4-ethylenedioxythiophene)-polystyrene sulfonate was added to the deionized water and stirred sufficiently to obtain a mixed solution I;

[0052] Step 2: Add 3 mL of ethylene glycol to the mixed solution I, and stir at 50° C. to obtain a mixed solution II;

[0053] Step 3: Add 0.1 g chitosan, 2 mL acrylic acid, and 3 mL 2-hydroxyethyl methacrylate monomer to the mixed solution II and stir thoroughly for 30 min at 50° C. until completely dissolved to obtain a mixed solution III;

[0054] Step 4: After the mixed solution III is cooled to 25°C, 1 mL of ammonium persulfate and 0.005 g of tannic acid are added, and stirred for 30 min until completely dissolved to obtain a mixed solution IV;

[0055] Step 5: Finally, the mixed solution IV is poured into a mold and free radical polymerized at 65°C for 4 hours to obtain a conductive hydrogel with environmental resistance and antifreeze properties.

[0056] Example 4

[0057] The preparation of the hydrogel with environmental resistance, antifreeze properties and electrical conductivity of this embodiment is carried out according to the following steps:

[0058] Step 1: First, 9 mL of deionized water was added to a beaker, and then 0.4 mL of poly(3,4-ethylenedioxythiophene)-polystyrene sulfonate was added to the deionized water and stirred sufficiently to obtain a mixed solution I;

[0059] Step 2: Add 1 mL of ethylene glycol to the mixed solution I, and stir at 50° C. to obtain a mixed solution II;

[0060] Step 3: Add 0.1 g chitosan, 2 mL acrylic acid, and 5 mL 2-hydroxyethyl methacrylate monomer to the mixed solution II and stir thoroughly for 30 min at 50° C. until completely dissolved to obtain a mixed solution III;

[0061] Step 4: After the mixed solution III is cooled to 25°C, 1 mL of ammonium persulfate and 0.005 g of tannic acid are added, and stirred for 30 min until completely dissolved to obtain a mixed solution IV;

[0062] Step 5: Finally, the mixed solution IV is poured into a mold and free radical polymerized at 65°C for 4 hours to obtain a conductive hydrogel with environmental resistance and antifreeze properties.

[0063] Example 5

[0064] The preparation of the hydrogel with environmental resistance, antifreeze properties and electrical conductivity of this embodiment is carried out according to the following steps:

[0065] Step 1: First, 7 mL of deionized water was added to a beaker, and then 1.0 mL of poly(3,4-ethylenedioxythiophene)-polystyrene sulfonate was added to the deionized water and stirred sufficiently to obtain a mixed solution I;

[0066] Step 2: Add 3 mL of ethylene glycol to the mixed solution I, and stir at 50° C. to obtain a mixed solution II;

[0067] Step 3: Add 0.1 g chitosan, 2 mL acrylic acid, and 5 mL 2-hydroxyethyl methacrylate monomer to the mixed solution II and stir thoroughly for 30 min at 50° C. until completely dissolved to obtain a mixed solution III;

[0068] Step 4: After the mixed solution III is cooled to 25°C, 1 mL of ammonium persulfate and 0.005 g of tannic acid are added, and stirred for 30 min until completely dissolved to obtain a mixed solution IV;

[0069] Step 5: Finally, the mixed solution IV is poured into a mold and free radical polymerized at 65°C for 4 hours to obtain a conductive hydrogel with environmental resistance and antifreeze properties.

[0070] Comparative Example 1

[0071] The preparation of the hydrogel of this comparative example was carried out according to the following steps:

[0072] Step 1: First, 7 mL of deionized water was added to a beaker, and then 0.4 mL of poly(3,4-ethylenedioxythiophene):polystyrene sulfonate was added to the deionized water and stirred thoroughly to obtain a mixed solution I;

[0073] Step 2: Add 3 mL of ethylene glycol to the mixed solution I, and stir at 50° C. to obtain a mixed solution II;

[0074] Step 3: Add 0.3 g chitosan, 2 mL acrylic acid, and 5 mL 2-hydroxyethyl methacrylate monomer to the mixed solution II and stir thoroughly for 30 min at 50° C. until completely dissolved to obtain a mixed solution III;

[0075] Step 4: After the mixed solution III is cooled to 25°C, 1 mL of ammonium persulfate and 0.005 g of tannic acid are added, and stirred for 30 min until completely dissolved to obtain a mixed solution IV;

[0076] Step 5: Finally, pour the mixed solution IV into a mold and perform free radical polymerization at 65 °C for 4 h.

[0077] Comparative Example 2

[0078] The preparation of the hydrogel of this comparative example was carried out according to the following steps:

[0079] Step 1: First, add 10 mL of deionized water into a beaker, then add 0.4 mL of poly(3,4-ethylenedioxythiophene):polystyrene sulfonate into the deionized water, and stir thoroughly at 50° C. to obtain a mixed solution I;

[0080] Step 2: Add 0.1 g chitosan, 2 mL acrylic acid, and 5 mL 2-hydroxyethyl methacrylate monomer to the mixed solution I and stir thoroughly at 50°C for 30 min until completely dissolved to obtain a mixed solution II.

[0081] Step 3: After the mixed solution II is cooled to 25°C, 1 mL of ammonium persulfate and 0.005 g of tannic acid are added, and stirred for 30 min until completely dissolved to obtain a mixed solution III;

[0082] Step 4: Finally, the mixed solution III was poured into a mold and free radical polymerized at 65 °C for 4 h.

[0083] Detection test

[0084] Figure 1 The swelling curves of the hydrogels prepared in Example 1 and Comparative Example 1 show that the double network structure formed by the introduction of chitosan makes the internal structure of the hydrogel more compact, thereby obtaining a more excellent anti-swelling performance. However, excessive chitosan will cause uneven cross-linking distribution inside the hydrogel, thereby weakening the anti-swelling performance.

[0085] Figure 2 1 and 2 are swelling curves of the hydrogels prepared in Example 1 and Example 2. Acrylic acid contains hydrophilic carboxylic acid groups. As the content of acrylic acid increases, the hydrophilicity increases and the anti-swelling property of the hydrogel decreases.

[0086] Figure 3 The swelling curves of the hydrogels prepared in Examples 1 and 3 show that as the content of 2-hydroxyethyl methacrylate increases, the content of hydrophobic ester groups increases, and thus the anti-swelling performance of the hydrogel is enhanced.

[0087] Figure 4 The swelling curves of the hydrogels prepared in Example 1 and Example 4 show that as the content of ethylene glycol increases, the number of hydrophilic hydroxyl groups in the hydrogel system increases, and thus the anti-swelling performance thereof weakens.

[0088] Figure 5 The swelling curves of the hydrogels prepared in Example 1 and Example 5 are shown. Poly(3,4-ethylenedioxythiophene)-polystyrene sulfonate is added to the hydrogel system as a conductive material to provide the hydrogel with conductive properties. However, excessive content of poly(3,4-ethylenedioxythiophene)-polystyrene sulfonate will lead to uneven distribution of substances in the system, thereby reducing the anti-swelling property of the hydrogel.

[0089] Figure 6 This is the swelling curve of the hydrogel prepared in Example 1 in different environments. It can be seen from the figure that the hydrogel has good anti-swelling properties in different environments (KCl, NaCl, C6H5O6, 65°C, 4°C), and the quality shows a shrinking trend.

[0090] Figure 7 The tensile stress-strain curves of the hydrogels prepared in Example 1 and Comparative Example 2 show that the hydrogel prepared with ethylene glycol (strain: 848.61% and stress 176.25 kPa) has better mechanical properties than the hydrogel prepared without ethylene glycol (strain: 693.76% and stress 151.67 kPa). This is mainly because ethylene glycol contains two hydroxyl groups that can form multiple hydrogen bonds with water molecules. A large number of hydrogen bonds give the hydrogel more excellent mechanical properties.

[0091] Figure 8 The tensile stress-strain curves of the hydrogel prepared in Example 1 under different temperatures. It can be seen from the figure that the mechanical properties are enhanced after freezing at -20°C and heating at 65°C. This is mainly due to the generation of more hydrogen bonds in the freezing environment and the enhanced fluidity between molecules in the 65°C environment. Therefore, the mechanical properties of the hydrogel are enhanced.

[0092] Fig. 9 The tensile stress-strain curves of the hydrogel prepared in Example 1 after being immersed in different environments. It can be seen that good mechanical properties are maintained in different solution environments. In particular, the mechanical strength is enhanced after being immersed in KCl (concentration of 0.2M) and NaCl (concentration of 0.2M) solutions for 15 days. This is mainly due to the trend of salting out, which makes the network structure denser and thus has stronger mechanical properties.

[0093] Fig.10 The signal output by the hydrogel prepared in Example 1 when attached to the wrist as a flexible wearable sensor in an underwater environment. It can be seen that the flexible wearable sensor has stability in monitoring human motion signals in an underwater environment.

[0094] The above are only preferred specific embodiments of the present invention, which are all different implementations based on the overall concept of the present invention, and the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A method for preparing a conductive hydrogel having environmental resistance and antifreeze properties, It is characterized in that The specific steps are: (1) adding poly(3,4-ethylenedioxythiophene)-polystyrene sulfonate into deionized water and stirring to obtain a mixed solution I; (2) adding ethylene glycol to the mixed solution I, and stirring at 50° C. to obtain a mixed solution II; (3) adding chitosan, acrylic acid, and 2-hydroxyethyl methacrylate monomer to the mixed solution II, and stirring thoroughly at 50° C. until completely dissolved, to obtain a mixed solution III; (4) cooling the mixed solution III, adding an aqueous solution of ammonium persulfate and tannic acid, stirring and dissolving to obtain a mixed solution IV; (5) Free radical polymerization of the mixed solution IV is performed to obtain a conductive hydrogel having environmental resistance and antifreeze properties.

2. The method for preparing the conductive hydrogel having environmental resistance and antifreeze properties according to claim 1, It is characterized in that Deionized water: poly(3.4-ethylenedioxythiophene)-polystyrene sulfonate: ethylene glycol: chitosan: acrylic acid: 2-hydroxyethyl methacrylate: aqueous ammonium persulfate solution: tannic acid = 7 ml: 0.4 ml: 3 ml: 0.1 g: 2 ml: 5 ml: 1 ml: 0.005 g.

3. The method for preparing the conductive hydrogel having environmental resistance and antifreeze properties according to claim 1, It is characterized in that The concentration of the ammonium persulfate aqueous solution is 60 mg / mL.

4. The method for preparing the conductive hydrogel having environmental resistance and antifreeze properties according to claim 1, It is characterized in that The temperature of free radical polymerization is 65°C and the time is 3-5h.

5. Conductive hydrogel with environmental resistance and antifreeze properties, It is characterized in that The method is prepared according to any one of claims 1 to 4.

6. Application of the environmentally resistant and antifreeze conductive hydrogel according to claim 5 in the field of flexible wearable sensor technology.