Production method of pigment carbon black with high screening property
Through high-temperature oxygen-rich air combustion, quenching of quenching water and multi-stage demagnetization treatment, the problem of high impurity content in traditional carbon black production is solved, and the production of pigmented carbon black with high cleanliness and excellent cross-net performance is achieved. It is suitable for Coloring of materials such as plastics and fibers.
Patent Information
- Application Number
- CN202411135333.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-07-23
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-26
AI Technical Summary
During the production process of traditional pigment carbon black, the presence of raw and auxiliary material impurities, inorganic salt ions and iron filings leads to a high content of impurities for finished carbon black, which easily blocks the filter net, reducing production efficiency and product performance.
Using high-temperature oxygen-rich air combustion, two quenching of quenching water, multi-stage demagnetization treatment and wet granulation, to ensure raw material purification and cleanliness of finished products, through gasification kettles, reactors, main bag filters and demagnetization Multi-step control of the mass machine removes impurities and ferromagnetic substances in carbon black.
It significantly reduces the impurity content and ash content in carbon black, improves the mesh performance, ensures excellent cleanliness and performance, and is suitable for the coloring of materials such as plastics and fibers.
Smart Images

Figure CN119019867A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of carbon black production, and in particular to a method for producing high-net-passing pigment carbon black. Background Art
[0002] Carbon black (also known as carbon black) is a kind of amorphous carbon. It is a black powder with low density and extremely fine particle size. It is a product obtained by incomplete combustion or thermal decomposition of hydrocarbon substances under insufficient air conditions. Pigment carbon black is a type of carbon black, generally used for coloring in inks, masterbatches, fibers, plastics and other products. According to the coloring strength and particle size, it is generally divided into four types: high-pigment carbon black, medium-pigment carbon black, ordinary-pigment carbon black and low-pigment carbon black. The addition of pigment carbon black can not only color the product, but also improve the weather resistance, wear resistance and other properties of the product, while reducing the cost of the product.
[0003] The traditional method of preparing pigment carbon black has a high content of inorganic salts, iron filings and other impurities in the finished carbon black due to impurities in the raw and auxiliary materials themselves, residual raw oil caused by incomplete reaction, generation of by-products during the reaction, introduction of inorganic salt ions in the quenching water, and iron filings generated due to friction during the production process. When used for coloring plastics, fibers, etc., the production filter is easily clogged, causing the pressure in front of the filter to rise rapidly, reducing production efficiency and affecting the performance of the product. Summary of the invention
[0004] The object of the present invention is to provide a method for producing high-net-passing pigment carbon black to solve the following technical problems:
[0005] (1) Due to the impurities in the raw materials, the residual raw oil caused by incomplete reaction, the generation of by-products during the reaction, the introduction of inorganic salt ions in the quenching water, and the generation of iron filings due to friction during the production process, the content of impurities such as inorganic salts and iron filings in the finished carbon black is relatively high;
[0006] (2) When used for coloring plastics, fibers, etc., the production filter is prone to clogging, causing the pressure in front of the filter to rise quickly, reducing production efficiency and affecting the performance of the product.
[0007] The purpose of the present invention can be achieved through the following technical solutions:
[0008] A method for producing high-net-passing pigment carbon black comprises the following steps:
[0009] S1, inputting the gasified raw oil, the filtered and impurity-removed natural gas and air into the combustion chamber;
[0010] S2, raw oil, natural gas and air are incompletely burned and cracked in the reactor to produce carbon black;
[0011] S3, the high temperature carbon black is quenched with water twice to obtain carbon black flue gas;
[0012] S4, carbon black flue gas enters the main bag filter, powdered carbon black is enriched on the main bag filter, and the carbon black is separated and collected by regular spraying, and then sent to the first demagnetizer by wind;
[0013] S5. The powdered carbon black after the first demagnetization enters the granulation system. The granulation method is wet granulation to obtain granular carbon black. The granular carbon black is dried in a dryer and then enters the second demagnetization machine.
[0014] S6. The granular carbon black after secondary demagnetization enters the finished product silo to be made into finished carbon black.
[0015] Preferably, in S1, the raw oil is anthracene oil with a water content of less than 0.5%; the anthracene oil is introduced into a gasification kettle for gasification at a gasification temperature of 300-350°C.
[0016] Preferably, in S1, the air is oxygen-enriched air with an oxygen content of ≥30%, and the oxygen-enriched air is preheated by an air preheater before entering the combustion chamber, and the preheating temperature is 700-800°C;
[0017] Specifically, after the oxygen-enriched air is filtered and impurities are removed, it is initially heat exchanged with the rapidly cooled carbon black flue gas in a tubular heat exchanger to save energy. It is then heated to 700-800°C and sent to the combustion chamber to ensure the purity of the raw oil and air in the combustion chamber. The advantage of using high-temperature oxygen-enriched air is that the reaction room temperature can be increased.
[0018] Preferably, in S2, the reactor is a high-temperature reactor, the cracking reaction temperature is 2000-2200°C, and the cracking residence time is 20 μs;
[0019] Specifically, the reaction in S2 is a closed reaction system, in which the incomplete combustion and cracking of the crude oil produce carbon black, and at the same time generate by-products such as polycyclic aromatic hydrocarbons. Due to the use of high-temperature oxygen-rich air, the reaction temperature of the system is as high as 2000-2200°C, which is conducive to the formation of the carbon black core, and has a good inhibitory effect on the residue of crude oil and the formation of intermediates, thereby ensuring the purity of the reaction process.
[0020] Preferably, in S3, the first rapid cooling water quenching uses desalted water, the spraying pressure is 1.0-1.5Mpa, and the carbon black flue gas is cooled to 740-760°C;
[0021] The second rapid cooling water quenching uses desalted water with a spray pressure of 0.7-1.0Mpa, and the carbon black flue gas is cooled to 240-260℃;
[0022] Specifically, the quenching water uses desalted water that does not contain inorganic salt ions, which avoids the adhesion of inorganic salts in the water on the surface of carbon black, resulting in increased ash content of carbon black and poor mesh passing performance. The quenching water nozzles are arranged in a Z shape to ensure sufficient mixing with the carbon black during spraying.
[0023] Preferably, in S4, when the carbon black enters the first demagnetizer, the temperature of the carbon black is 200-250°C;
[0024] Specifically, the carbon black after rapid cooling is enriched on the surface of the main bag filter, and powdered carbon black is obtained after regular blowing. The high-temperature flue gas is first exchanged with oxygen-rich air, and the waste heat is fully utilized and then used for power generation. The powdered carbon black is sent to the first demagnetizer to remove ferromagnetic substances caused by friction with equipment and pipelines. The temperature of the powdered carbon black entering the demagnetizer is relatively high, at 200-250°C. Carbon black at a higher temperature has better fluidity, which is conducive to the removal of magnetic substances.
[0025] Preferably, in S5, the carbon black entering the second demagnetizer is granular carbon black;
[0026] Specifically, granular carbon black is conducive to subsequent application and addition. The granulation adopts wet granulation with water as the medium. After drying, the granular carbon black is sent to the second demagnetizer to further remove the ferromagnetic substances in the carbon black, improve the cleanliness and screen performance;
[0027] Preferably, in S6, when the carbon black enters the finished product silo, the temperature of the carbon black is less than 50°C; specifically, low-temperature packaging of the finished carbon black product is conducive to quality stability.
[0028] Beneficial effects of the present invention:
[0029] (1) The present invention controls the content of impurities that affect the screen-passing performance in the finished carbon black from multiple aspects such as purification of raw materials and auxiliary materials, process control and demagnetization of finished products, specifically including gasification of raw oil, use of oxygen-enriched air, high-temperature preheating of oxygen-enriched air, high temperature of the reaction section, rapid cooling spray using desalted water, multi-stage removal of ferromagnetic impurities, etc., to produce pigment carbon black with high screen-passing performance. The pigment carbon black has few impurities and high cleanliness, with a 325-mesh sieve residue of less than 50ppm, ash content ≤0.1%, toluene transmittance ≥98%, and polycyclic aromatic hydrocarbon content ≤10ppm. After being used to prepare a masterbatch with a carbon black content of 35%, the filtration pressure rise value tested according to the standard is ≤2MPa (the filter screen is 1400 mesh), and the screen-passing performance is excellent;
[0030] (2) After filtering and removing impurities, the oxygen-enriched air of the present invention is initially heat-exchanged with the carbon black flue gas after rapid cooling in a tubular heat exchanger to save energy consumption, and then heated to 700-800°C and sent to the combustion chamber to ensure the purity of the raw oil and air in the combustion chamber. The advantage of using high-temperature oxygen-enriched air is that the reaction room temperature can be increased;
[0031] (3) In the present invention, the incomplete combustion and cracking of the raw oil produce carbon black, and at the same time generate by-products such as polycyclic aromatic hydrocarbons. Due to the use of high-temperature oxygen-rich air, the reaction temperature of the system is as high as 2000-2200°C, which is conducive to the formation of the carbon black core, has a good inhibitory effect on the residue of the raw oil and the formation of intermediates, and ensures the purity of the reaction process;
[0032] (4) The carbon black after rapid cooling in the present invention is enriched on the surface of the main bag filter, and powdered carbon black is obtained after regular purging. The high-temperature flue gas is first heat-exchanged with oxygen-enriched air, and the waste heat is fully utilized and then used for power generation. The powdered carbon black is sent to the first demagnetizer to remove ferromagnetic substances generated by friction with equipment and pipelines. The temperature of the powdered carbon black entering the demagnetizer is relatively high, at 200-250°C. Carbon black at a higher temperature has better fluidity, which is conducive to the removal of magnetic substances.
[0033] (5) The granulation of the present invention adopts wet granulation using water as the medium. After the granular carbon black is dried, it is sent to the second demagnetizer to further remove the ferromagnetic substances in the carbon black, thereby improving the cleanliness and screen passing performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] The present invention will be further described below in conjunction with the accompanying drawings.
[0035] Figure 1 It is a production process diagram of a method for producing high-net-passing pigment carbon black of the present invention;
[0036] Figure 2 It is a working schematic diagram of a demagnetizer in a method for producing high-net-passing pigment carbon black of the present invention;
[0037] Figure 3 This is an electron microscope image of the distribution of the pigment carbon black in the PA6 masterbatch of the present invention. DETAILED DESCRIPTION
[0038] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0039] Example 1
[0040] See also Figure 1-Figure 3 As shown, the present invention is a method for producing high-net-passing pigment carbon black, comprising the following steps:
[0041] S1, inputting the gasified raw oil, the filtered and impurity-removed natural gas and air into the combustion chamber;
[0042] Specifically, in this embodiment, the raw material oil is anthracene oil with a water content of 0.1%. The anthracene oil is introduced into a gasification kettle for gasification at a gasification temperature of 350°C.
[0043] The air is oxygen-enriched air with an oxygen content of 35%. The oxygen-enriched air is preheated by an air preheater before entering the combustion chamber. The preheating temperature is 700°C.
[0044] S2, raw oil, natural gas and air are incompletely burned and cracked in the reactor to produce carbon black;
[0045] Specifically, in this embodiment, the reactor is a high-temperature reactor, the cracking reaction temperature is 2000°C, and the cracking residence time is 20 μs;
[0046] S3, the high temperature carbon black is quenched with water twice to obtain carbon black flue gas;
[0047] Specifically, in this embodiment, the first rapid cooling water quenching uses desalted water, the spraying pressure is 1.3Mpa, and the carbon black flue gas is cooled to 750°C;
[0048] The second rapid cooling water quenching uses desalted water with a spray pressure of 1.0 MPa, and the carbon black flue gas is cooled to 250°C.
[0049] S4, carbon black flue gas enters the main bag filter, powdered carbon black is enriched on the main bag filter, and the carbon black is separated and collected by regular spraying, and then sent to the first demagnetizer by wind;
[0050] Specifically, in this embodiment, when the carbon black enters the first demagnetizer, the temperature of the carbon black is 250°C;
[0051] S5. The powdered carbon black after the first demagnetization enters the granulation system. The granulation method is wet granulation to obtain granular carbon black. The granular carbon black is dried in a dryer and then enters the second demagnetization machine.
[0052] Specifically, in this embodiment, the carbon black entering the second demagnetizer is granular carbon black;
[0053] S6, the granular carbon black after secondary demagnetization enters the finished product silo to be made into finished carbon black;
[0054] Specifically, in this embodiment, when the carbon black enters the finished product silo, the temperature of the carbon black is 35°C.
[0055] After testing, the finished carbon black has a 325-mesh sieve residue of 48ppm, ash content of 0.08%, toluene transmittance of 98.2%, and polycyclic aromatic hydrocarbon content of 10ppm, indicating that the carbon black has high cleanliness, low content of raw material residue and reaction by-products, low content of sieve residue, and good mesh passing performance. After the carbon black and PA6 slices are mixed and granulated at a mass ratio of 35:65, the filtration pressure rise value is tested by the standard method to be 1.8MPa (the filter is 1400 mesh), and the measured mesh passing performance is good.
[0056] Example 2
[0057] A method for producing high-net-passing pigment carbon black comprises the following steps:
[0058] S1, inputting the gasified raw oil, the filtered and impurity-removed natural gas and air into the combustion chamber;
[0059] Specifically, in this embodiment, the raw material oil is anthracene oil with a water content of 0.15%. The anthracene oil is passed into a gasification kettle for gasification at a gasification temperature of 350°C.
[0060] The air is oxygen-enriched air with an oxygen content of 40%. The oxygen-enriched air is preheated by an air preheater before entering the combustion chamber. The preheating temperature is 750°C.
[0061] S2, raw oil, natural gas and air are incompletely burned and cracked in the reactor to produce carbon black;
[0062] Specifically, in this embodiment, the reactor is a high-temperature reactor, the cracking reaction temperature is 2050°C, and the cracking residence time is 20μs;
[0063] S3, the high temperature carbon black is quenched with water twice to obtain carbon black flue gas;
[0064] Specifically, in this embodiment, the first rapid cooling water quenching uses desalted water, the spraying pressure is 1.3Mpa, and the carbon black flue gas is cooled to 750°C;
[0065] The second rapid cooling water quenching uses desalted water with a spray pressure of 1.0 MPa, and the carbon black flue gas is cooled to 250°C.
[0066] S4, carbon black flue gas enters the main bag filter, powdered carbon black is enriched on the main bag filter, and the carbon black is separated and collected by regular spraying, and then sent to the first demagnetizer by wind;
[0067] Specifically, in this embodiment, when the carbon black enters the first demagnetizer, the temperature of the carbon black is 250°C;
[0068] S5. The powdered carbon black after the first demagnetization enters the granulation system. The granulation method is wet granulation to obtain granular carbon black. The granular carbon black is dried in a dryer and then enters the second demagnetization machine.
[0069] Specifically, in this embodiment, the carbon black entering the second demagnetizer is granular carbon black;
[0070] S6, the granular carbon black after secondary demagnetization enters the finished product silo to be made into finished carbon black;
[0071] Specifically, in this embodiment, when the carbon black enters the finished product silo, the temperature of the carbon black is 35°C.
[0072] After testing, the finished carbon black has a 325-mesh sieve residue of 48ppm, ash content of 0.08%, toluene transmittance of 98.7%, and polycyclic aromatic hydrocarbon content of 8ppm, indicating that the carbon black has high cleanliness, low content of raw material residue and reaction by-products, low content of sieve residue, and theoretically good mesh performance. After the carbon black and PA6 slices are mixed and granulated at a mass ratio of 35:65, the filtration pressure rise value is tested by the standard method to be 1.8MPa (the filter is 1400 mesh), and the actual mesh performance is good.
[0073] Example 3
[0074] The present invention is a method for producing high-net-passing pigment carbon black, comprising the following steps:
[0075] S1, inputting the gasified raw oil, the filtered and impurity-removed natural gas and air into the combustion chamber;
[0076] Specifically, in this embodiment, the raw material oil is anthracene oil with a water content of 0.1%. The anthracene oil is introduced into a gasification kettle for gasification at a gasification temperature of 350°C.
[0077] The air is oxygen-enriched air with an oxygen content of 40%. The oxygen-enriched air is preheated by an air preheater before entering the combustion chamber. The preheating temperature is 800°C.
[0078] S2, raw oil, natural gas and air are incompletely burned and cracked in the reactor to produce carbon black;
[0079] Specifically, in this embodiment, the reactor is a high-temperature reactor, the cracking reaction temperature is 2100°C, and the cracking residence time is 20 μs;
[0080] S3, the high temperature carbon black is quenched with water twice to obtain carbon black flue gas;
[0081] Specifically, in this embodiment, the first rapid cooling water quenching uses desalted water, the spraying pressure is 1.3Mpa, and the carbon black flue gas is cooled to 750°C;
[0082] The second rapid cooling water quenching uses desalted water with a spray pressure of 1.0 MPa, and the carbon black flue gas is cooled to 250°C.
[0083] S4, carbon black flue gas enters the main bag filter, powdered carbon black is enriched on the main bag filter, and the carbon black is separated and collected by regular spraying, and then sent to the first demagnetizer by wind;
[0084] Specifically, in this embodiment, when the carbon black enters the first demagnetizer, the temperature of the carbon black is 250°C;
[0085] S5. The powdered carbon black after the first demagnetization enters the granulation system. The granulation method is wet granulation to obtain granular carbon black. The granular carbon black is dried in a dryer and then enters the second demagnetization machine.
[0086] Specifically, in this embodiment, the carbon black entering the second demagnetizer is granular carbon black;
[0087] S6, the granular carbon black after secondary demagnetization enters the finished product silo to be made into finished carbon black;
[0088] Specifically, in this embodiment, when the carbon black enters the finished product silo, the temperature of the carbon black is 35°C.
[0089] After testing, the finished carbon black has a 325-mesh sieve residue of 46ppm, ash content of 0.07%, toluene transmittance of 98.9%, and polycyclic aromatic hydrocarbon content of 7ppm, indicating that the carbon black has high cleanliness, low content of raw material residue and reaction by-products, low content of sieve residue, and theoretically good mesh performance. After the carbon black and PA6 slices are mixed and granulated at a mass ratio of 35:65, the filtration pressure rise value is tested by standard methods and is 1.6MPa (the filter is 1400 mesh), and the actual mesh performance is good.
[0090] Example 4
[0091] A method for producing high-net-passing pigment carbon black comprises the following steps:
[0092] S1, inputting the gasified raw oil, the filtered and impurity-removed natural gas and air into the combustion chamber;
[0093] Specifically, in this embodiment, the raw material oil is anthracene oil with a water content of 0.4%. The anthracene oil is introduced into a gasification kettle for gasification at a gasification temperature of 300°C.
[0094] The air is oxygen-enriched air with an oxygen content of 30%. The oxygen-enriched air is preheated by an air preheater before entering the combustion chamber. The preheating temperature is 700-800℃.
[0095] S2, raw oil, natural gas and air are incompletely burned and cracked in the reactor to produce carbon black;
[0096] Specifically, in this embodiment, the reactor is a high-temperature reactor, the cracking reaction temperature is 2200°C, and the cracking residence time is 20 μs;
[0097] S3, the high temperature carbon black is quenched with water twice to obtain carbon black flue gas;
[0098] Specifically, in this embodiment, the first rapid cooling water quenching uses desalted water, the spraying pressure is 1.0 MPa, and the carbon black flue gas is cooled to 740°C;
[0099] The second rapid cooling water quenching uses desalted water with a spray pressure of 0.7 MPa, and the carbon black flue gas is cooled to 240°C.
[0100] S4, carbon black flue gas enters the main bag filter, powdered carbon black is enriched on the main bag filter, and the carbon black is separated and collected by regular spraying, and then sent to the first demagnetizer by wind;
[0101] Specifically, in this embodiment, when the carbon black enters the first demagnetizer, the temperature of the carbon black is 200°C;
[0102] S5. The powdered carbon black after the first demagnetization enters the granulation system. The granulation method is wet granulation to obtain granular carbon black. The granular carbon black is dried in a dryer and then enters the second demagnetization machine.
[0103] Specifically, in this embodiment, the carbon black entering the second demagnetizer is granular carbon black;
[0104] S6, the granular carbon black after secondary demagnetization enters the finished product silo to be made into finished carbon black;
[0105] Specifically, in this embodiment, when the carbon black enters the finished product silo, the temperature of the carbon black is 40°C.
[0106] After testing, the finished carbon black has a 325-mesh sieve residue of 46ppm, ash content of 0.08%, toluene transmittance of 98.6%, and polycyclic aromatic hydrocarbon content of 8ppm, indicating that the carbon black has high cleanliness, low content of raw material residue and reaction by-products, low content of sieve residue, and theoretically good mesh performance. After the carbon black and PA6 slices are mixed and granulated at a mass ratio of 35:65, the filtration pressure rise value is tested by the standard method to be 1.7MPa (the filter is 1400 mesh), and the actual mesh performance is good.
[0107] Example 5
[0108] A method for producing high-net-passing pigment carbon black comprises the following steps:
[0109] S1, inputting the gasified raw oil, the filtered and impurity-removed natural gas and air into the combustion chamber;
[0110] Specifically, in this embodiment, the raw material oil is anthracene oil, and the water content is less than 0.5%. The anthracene oil is passed into a gasification kettle for gasification, and the gasification temperature is 320°C;
[0111] The air is oxygen-enriched air with an oxygen content of 30%. The oxygen-enriched air is preheated by an air preheater before entering the combustion chamber. The preheating temperature is 700°C.
[0112] S2, raw oil, natural gas and air are incompletely burned and cracked in the reactor to produce carbon black;
[0113] Specifically, in this embodiment, the reactor is a high-temperature reactor, the cracking reaction temperature is 2200°C, and the cracking residence time is 20 μs;
[0114] S3, the high temperature carbon black is quenched with water twice to obtain carbon black flue gas;
[0115] Specifically, in this embodiment, the first rapid cooling water quenching uses desalted water, the spraying pressure is 1.5 MPa, and the carbon black flue gas is cooled to 760°C;
[0116] The second rapid cooling water quenching uses desalted water with a spray pressure of 0.8Mpa, and the carbon black flue gas is cooled to 260℃.
[0117] S4, carbon black flue gas enters the main bag filter, powdered carbon black is enriched on the main bag filter, and the carbon black is separated and collected by regular spraying, and then sent to the first demagnetizer by wind;
[0118] Specifically, in this embodiment, when the carbon black enters the first demagnetizer, the temperature of the carbon black is 220°C;
[0119] S5. The powdered carbon black after the first demagnetization enters the granulation system. The granulation method is wet granulation to obtain granular carbon black. The granular carbon black is dried in a dryer and then enters the second demagnetization machine.
[0120] Specifically, in this embodiment, the carbon black entering the second demagnetizer is granular carbon black;
[0121] S6, the granular carbon black after secondary demagnetization enters the finished product silo to be made into finished carbon black;
[0122] Specifically, in this embodiment, when the carbon black enters the finished product silo, the temperature of the carbon black is 40°C.
[0123] After testing, the finished carbon black has a 325-mesh sieve residue of 47ppm, ash content of 0.06%, toluene transmittance of 98.8%, and polycyclic aromatic hydrocarbon content of 7ppm, indicating that the carbon black has high cleanliness, low content of raw material residue and reaction by-products, low content of sieve residue, and theoretically good mesh performance. After the carbon black and PA6 slices are mixed and granulated at a mass ratio of 35:65, the filtration pressure rise value is tested by the standard method to be 1.5MPa (the filter is 1400 mesh), and the actual mesh performance is good.
[0124] The above is a detailed description of an embodiment of the present invention, but the content is only a preferred embodiment of the present invention and cannot be considered to limit the scope of implementation of the present invention. All equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.
Claims
1. A method for producing high-net-passing pigment carbon black, characterized in that: The steps include: S1, inputting the gasified raw oil, the filtered and impurity-removed natural gas and air into the combustion chamber; S2, raw oil, natural gas and air are incompletely burned and cracked in the reactor to produce carbon black; S3, the high temperature carbon black is quenched with water twice to obtain carbon black flue gas; S4, carbon black flue gas enters the main bag filter, powdered carbon black is enriched on the main bag filter, and the carbon black is separated and collected by regular spraying, and then sent to the first demagnetizer by wind; S5, the powdered carbon black after the first demagnetization enters the granulation system to obtain granular carbon black, and the granular carbon black enters the second demagnetization machine after being dried in the dryer; S6. The granular carbon black after secondary demagnetization enters the finished product silo to be made into finished carbon black.
2. The method for producing high-net-passing pigment carbon black according to claim 1, characterized in that: In S1, the raw oil is anthracene oil with a water content of less than 0.5%; the anthracene oil is gasified in a gasifier at a gasification temperature of 300-350°C.
3. The method for producing high-net-passing pigment carbon black according to claim 2, characterized in that: In S1, the air is oxygen-enriched air, and the oxygen content is ≥30%.
4. The method for producing high-net-passing pigment carbon black according to claim 3, characterized in that: The oxygen-enriched air is preheated in an air preheater before entering the combustion chamber, and the preheating temperature is 700-800°C.
5. The method for producing high-net-passing pigment carbon black according to claim 1, characterized in that: In S2, the reactor is a high-temperature reactor, the cracking reaction temperature is 2000-2200°C, and the cracking residence time is 20 μs.
6. The method for producing high-net-passing pigment carbon black according to claim 1, characterized in that: In S3, the first rapid cooling water quenching uses desalted water, the spraying pressure is 1.0-1.5Mpa, and the carbon black flue gas is cooled to 740-760°C.
7. The method for producing high-net-passing pigment carbon black according to claim 6, characterized in that: In S3, the second rapid cooling water quenching uses desalted water, the spraying pressure is 0.7-1.0 MPa, and the carbon black flue gas is cooled to 240-260°C.
8. The method for producing high-net-passing pigment carbon black according to claim 1, characterized in that: In S4, when the carbon black enters the first demagnetizer, the temperature of the carbon black is 200-250°C.
9. The method for producing high-net-passing pigment carbon black according to claim 8, characterized in that: In S4, the carbon black after rapid cooling is enriched on the surface of the main bag filter, and powdered carbon black is obtained after regular blowing, and the powdered carbon black is sent to the first demagnetizer.
10. The method for producing high-net-passing pigment carbon black according to claim 1, characterized in that: In S5, the granulator uses water as a medium to perform wet granulation.