Diamond wire cutting fluid and preparation method and application thereof
Through the diamond wire cutting liquid composed of block polyether lubricant, polyether wetting agent and polyether leveling agent with specific ratios, the edge collapse problem during silicon wafer cutting is solved, and the cutting efficiency and product are improved quality.
Patent Information
- Application Number
- CN202411153882.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-26
AI Technical Summary
During the cutting process of large-size silicon wafers, the difference in thermal expansion coefficient between the diamond wire saw and the silicon wafer leads to edge collapse problems, affecting production efficiency and product quality.
Using diamond wire cutting liquid composed of block polyether lubricants, polyether wetting agents and polyether leveling agents, the preparation of specific mass ratios and mass average molecular weights is formed to form low dynamic surface tension and improve wetting. Effects, reduce friction and heat generation, and reduce the risk of edge collapse.
It significantly improves the edge collapse during cutting of large-size silicon wafers, improves yield, and reduces quality problems caused by wear and thermal expansion.
Smart Images

Figure CN119020088A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a diamond wire cutting liquid and a preparation method and application thereof, belonging to the field of semiconductors. Background Art
[0002] In industries such as semiconductors and photovoltaics, the cutting of large-size silicon wafers is a critical processing step. The cut silicon wafers are used to manufacture solar cells and semiconductor chips, so their quality and processing efficiency are crucial to the performance and cost of the final product. Usually, in order to obtain silicon wafers of the required size, people use diamond wire or emery wire for cutting.
[0003] With the advancement of thinning and slicing, the glue layer and resin plate layer in direct contact with the silicon rod are becoming thinner and thinner. As the glue layer and the resin plate become thinner and thinner, the diamond wire saw rubs violently with the three components of single crystal silicon-glue-resin plate at the finishing depth, and the glue layer has a greater deformation. Due to the difference in thermal expansion coefficients between glue and single crystal silicon, the thinner silicon wafers at the finishing point are more prone to edge collapse, causing losses to production activities.
[0004] Therefore, it is urgent to develop a new type of diamond wire cutting fluid to solve the edge collapse problem when cutting large-size silicon wafers. Summary of the invention
[0005] The invention provides a diamond wire cutting liquid, which can effectively improve the edge collapse problem when being used for cutting large-size silicon wafers.
[0006] The present invention also provides a method for preparing a diamond wire cutting fluid. The method is simple to operate, and the diamond wire cutting fluid prepared according to the method can effectively improve the edge collapse problem when used for cutting large-size silicon wafers.
[0007] The present invention also provides a silicon wafer cutting method, which uses the diamond wire cutting liquid to cut the silicon wafer, and can effectively improve the problem of edge collapse during the cutting process.
[0008] On one hand, the present invention provides a diamond wire cutting fluid, comprising functional components and water; the functional components comprise 20-30 parts by mass of a block polyether lubricant, 10-15 parts by mass of a polyether wetting agent, and 1-5 parts by mass of a polyether leveling agent; the mass average molecular weight of the block polyether lubricant is 2000-6000, the mass average molecular weight of the polyether wetting agent is 100-1000, and the mass average molecular weight of the polyether leveling agent is not higher than 4000; the polyether leveling agent comprises at least one of fluorine-modified polyether, silicon-modified polyether, and bridge structure polyether; the mass ratio of the functional components to the water is 2:5.
[0009] In the diamond wire cutting fluid as described above, the functional components include 24-26 parts by mass of block polyether lubricant, 12-14 parts by mass of polyether wetting agent, and 3-4 parts by mass of polyether leveling agent.
[0010] In the diamond wire cutting fluid as described above, the mass average molecular weight of the block polyether lubricant is 2000-4000.
[0011] In the diamond wire cutting fluid as described above, the mass average molecular weight of the polyether wetting agent is 300-800.
[0012] In the diamond wire cutting fluid as described above, the surface tension of the block polyether lubricant is 40-50 mN / m; and / or, the surface tension of the polyether wetting agent is 30-35 mN / m; and / or, the surface tension of the polyether leveling agent is not higher than 25 mN / m.
[0013] In the diamond wire cutting fluid as described above, the block polyether lubricant is a random block polyether lubricant.
[0014] In the diamond wire cutting fluid as described above, the molar amount of the branched chains of the polyether compound in the polyether wetting agent is greater than 40%.
[0015] In another aspect, the present invention provides a method for preparing the diamond wire cutting fluid as described above, comprising the following steps: mixing a block polyether lubricant, a polyether wetting agent, and a polyether leveling agent, then adding water and stirring for 3-4 hours, and aging for 1 hour to obtain the diamond wire cutting fluid.
[0016] In the preparation method as described above, during the mixing, the stirring speed is 1000-1500 rpm and the stirring time is 30-60 min.
[0017] Another aspect of the present invention provides a silicon wafer cutting method, which uses the diamond wire cutting liquid as described above or the diamond wire cutting liquid prepared according to the preparation method as described above to cut the silicon wafer.
[0018] The diamond wire cutting fluid provided by the present invention is composed of a block polyether lubricant with a specific mass average molecular weight, a polyether wetting agent and a polyether leveling agent in specific weight portions, and can give full play to the synergistic effect between the three types of components. When used for cutting large-size silicon wafers, it can significantly improve the edge collapse and improve the yield rate. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is a picture of a silicon wafer cut by the diamond wire cutting fluid provided in Example 3 of the present invention;
[0020] Figure 2 This is a picture of a silicon wafer cut by the diamond wire cutting fluid provided in Comparative Example 4 of the present invention. DETAILED DESCRIPTION
[0021] In order to make the purpose, technical solutions and advantages of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0022] On one hand, the present invention provides a diamond wire cutting fluid, comprising functional components and water; the functional components comprise 20-30 parts by mass of a block polyether lubricant, 10-15 parts by mass of a polyether wetting agent, and 1-5 parts by mass of a polyether leveling agent; the mass average molecular weight of the block polyether lubricant is 2000-6000, the mass average molecular weight of the polyether wetting agent is 100-1000, and the mass average molecular weight of the polyether leveling agent is not higher than 4000; the polyether leveling agent comprises at least one of fluorine-modified polyether, silicon-modified polyether, and bridge structure polyether; and the mass ratio of the functional components to water is 2:5.
[0023] The diamond wire cutting fluid provided by the present invention is composed of a block polyether lubricant with a specific mass average molecular weight, a polyether wetting agent, a polyether leveling agent and water in certain parts by mass, and can effectively improve the edge collapse problem in the process of cutting large-size silicon wafers.
[0024] In detail, the mass parts of the block polyether lubricant in the functional component include but are not limited to 20 parts, 21 parts, 22 parts, 23 parts, 24 parts, 25 parts, 26 parts, 27 parts, 28 parts, 29 parts, 30 parts or a range composed of any two parts thereof.
[0025] The polyether wetting agent includes but is not limited to 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, 15 parts or a range between any two parts.
[0026] The polyether leveling agent includes, but is not limited to, 1 part, 1.5 parts, 2 parts, 2.5 parts, 3 parts, 3.5 parts, 4 parts, 4.5 parts, 5 parts or a range between any two of them.
[0027] The mass average molecular weight of the block polyether lubricant is 2000-6000. The appropriate type of block polyether lubricant meeting the above mass average molecular weight can be selected according to actual needs. For example, the block polyether lubricant can be selected from block polyether lubricants of models such as 1740, PE6400, PE3100, PE6100, 1720, and GPE-3000.
[0028] The mass average molecular weight of the polyether wetting agent is 100-1000. The appropriate type of polyether wetting agent meeting the above mass average molecular weight can be selected according to actual needs. For example, the polyether wetting agent can be BASF XP-90, BASF XP-40 and other models of polyether wetting agents.
[0029] The mass average molecular weight of the polyether leveling agent is not higher than 4000. Similarly, a suitable type of polyether leveling agent meeting the above mass average molecular weight can be selected according to actual needs.
[0030] The polyether leveling agent includes at least one of fluorine-modified polyether, silicon-modified polyether and bridge structure polyether.
[0031] Specifically, fluorine-modified polyether refers to a ring body substituted by monofluoroalkyl, difluoroalkyl, or perfluoroalkyl, in which the fluoroalkyl group is retained on the side chain of polyoxyethylene ether, and the fluoroalkyl side chain accounts for 3-8% of the molecular weight; silicon-modified polyether refers to a polydimethylsiloxane acrylate graft copolymer; bridge structure polyether refers to a type of gemini surfactant in which two polyether segments are connected by a linking group, and the linking group can be an ethylene group (-CH 2 -CH 2 -), propylene (-CH 2 -CH 2 -CH 2 -), alkynyl (-C≡C-).
[0032] In a specific implementation, the polyether leveling agent can be DuPont Zonoyl FSO, EFKA-3580, BYK-306, non-silicone leveling agent Surfony 104 and other types of polyether leveling agents.
[0033] In another specific embodiment, the polyether leveling agent is a silicon-modified polyether, which has an organic siloxane as the main chain and has excellent compatibility with 10-20 μm silicon powder, and can disperse silicon powder particles from the aggregated state, reduce the particle size of the aggregated state of silicon powder, and disperse the silicon powder in the circulating working fluid. In the final stage of cutting, it can prevent the silicon powder from directly acting as abrasive particles and avoid generating a large amount of heat when cutting the glue layer.
[0034] The diamond wire cutting fluid provided by the present invention can effectively improve the edge collapse problem in the process of cutting large-size silicon wafers. The inventors have found through a large number of creative experiments that the surface tension of the diamond wire cutting fluid provided by the present invention can reach 27mN / m at a working fluid concentration of 0.5%-1% by mass at 1000ms, which means that the diamond wire cutting fluid provided by the present invention has a lower dynamic surface tension. When the diamond wire saw cuts single crystal silicon at high speed, according to the Young-Dure equation:
[0035] S=γ LV (cosθ-1)
[0036] S is the spreading coefficient, a parameter to measure the wetting effect; γ LV is the free energy of the liquid-gas interface (equivalent to the measured dynamic surface tension of the liquid); θ is the contact angle of the liquid on the surface of the solid material. The condition for the equation to have physical significance is S < 0. The spreading coefficient is inversely proportional to the dynamic surface tension. A lower dynamic surface tension can show a better wetting and penetration effect. In particular, it has a better cooling effect on the glue layer at the end cutting depth and reduces the occurrence of edge collapse.
[0037] Furthermore, in a specific embodiment of the present invention, the functional components include 24-26 parts by weight of block polyether lubricant, 12-14 parts by weight of polyether wetting agent, and 3-4 parts by weight of polyether leveling agent.
[0038] In detail, the block polyether lubricant includes but is not limited to 24 parts, 24.2 parts, 24.6 parts, 24.8 parts, 25 parts, 25.2 parts, 25.4 parts, 25.6 parts, 25.8 parts, 26 parts or a range between any two of them.
[0039] The polyether wetting agent includes but is not limited to 12 parts, 12.2 parts, 12.4 parts, 12.6 parts, 12.8 parts, 13.0 parts, 13.2 parts, 13.4 parts, 13.6 parts, 13.8 parts, 14 parts or a range between any two of them.
[0040] The polyether leveling agent includes but is not limited to 3 parts, 3.2 parts, 3.4 parts, 3.6 parts, 3.8 parts, 4.0 parts or a range between any two of them.
[0041] When the functional components are formulated in the above-mentioned mass parts range, the diamond wire cutting fluid has a better yield rate. The inventors analyzed that the reason may be that when the diamond wire cutting fluid is composed of mass parts in the above-mentioned range, it can achieve a lower dynamic surface tension and achieve a better cutting effect.
[0042] Furthermore, in a specific embodiment of the present invention, the mass average molecular weight of the block polyether lubricant is 2000-4000.
[0043] Specifically, the mass average molecular weight of the block polyether lubricant includes, but is not limited to, 2000, 2500, 3000, 3500, 4000 or a range between any two of these.
[0044] When the mass average molecular weight of the block polyether lubricant is within the above range, the diamond wire cutting fluid can better reduce the occurrence of edge chipping when used to cut silicon wafers. The inventors analyzed that the reason may be that when the block polyether lubricant meeting the above mass average molecular weight is used in the diamond wire cutting fluid, it can further reduce the friction between the diamond wire and the silicon wafer, reduce wear, and thus reduce the occurrence of edge chipping.
[0045] Furthermore, in a specific embodiment of the present invention, the mass average molecular weight of the polyether wetting agent is 300-800.
[0046] In detail, the mass average molecular weight of the polyether wetting agent includes but is not limited to 300, 400, 500, 600, 700, 800 or a range between any two thereof.
[0047] When the mass average molecular weight of the polyether wetting agent is within the above range, the diamond wire cutting fluid can better reduce the occurrence of edge chipping when used in cutting silicon wafers. The inventors analyzed that the reason may be that the polyether wetting agent that meets the above mass average molecular weight can further improve the wetting and liquid carrying ability of the diamond wire cutting fluid when used in the diamond wire cutting fluid, effectively reduce the heat generated during the cutting process, improve the cutting ability of the diamond wire, and thus reduce the occurrence of edge chipping.
[0048] Further, in a specific embodiment of the present invention, the surface tension of the block polyether lubricant is 40-50 mN / m; and / or, the surface tension of the polyether wetting agent is 30-35 mN / m; and / or, the surface tension of the polyether leveling agent is not higher than 25 mN / m.
[0049] The surface tension of block polyether lubricants, polyether wetting agents and polyether leveling agents refers to the static surface tension, which can be measured by the maximum bubbling pressure method ( Dynamic surface tension was measured by a surface tension meter.
[0050] In detail, the surface tension of the block polyether lubricant includes but is not limited to 40 mN / m, 42 mN / m, 44 mN / m, 46 mN / m, 48 mN / m, 50 mN / m or a range between any two thereof.
[0051] The surface tension of the polyether wetting agent includes but is not limited to 30 mN / m, 31 mN / m, 32 mN / m, 33 mN / m, 34 mN / m, 35 mN / m or a range between any two of them.
[0052] The surface tension of the polyether leveling agent is not higher than 25 mN / m. For example, the surface tension of the polyether leveling agent includes but is not limited to 25 mN / m, 24 mN / m, 23 mN / m, 22 mN / m, 21 mN / m, 20 mN / m, 19 mN / m, 18 mN / m or any other range not higher than 25 mN / m.
[0053] When the surface tension of the polyether wetting agent or the surface tension of the polyether leveling agent is within the above range, a gradient surface tension change can be provided, thereby improving the stability and synergy between the various components of the diamond wire cutting fluid.
[0054] Furthermore, in a specific embodiment of the present invention, the block polyether lubricant is a random block polyether lubricant.
[0055] The random block polyether lubricant of the present invention is a random copolymer of ethylene oxide (EO) and propylene oxide (PO) through a one-step catalytic ring-opening polymerization, such as glycerol random polyether GPE-3000 and butanol random polyether BPE-2500.
[0056] Due to the introduction of PO groups, this type of EO / EO random polyether has more side chains than PEG series copolymers. These side chains can provide a certain hydrophobic effect and steric hindrance, causing slippage between polyether lubricant molecules and providing macroscopic slippage. Moreover, EO / PO block polyether has an appropriate cloud point at a certain number of PO side chains. The heat of diamond wire saw friction makes the cutting reach the cloud point, and the polyether precipitates, wraps the steel wire, and produces oil film lubrication.
[0057] Furthermore, in one embodiment of the present invention, the molar amount of the branched chains of the polyether compound in the polyether wetting agent is greater than 40%.
[0058] Specifically, the branched chains of the polyether compound in the polyether wetting agent refer to all chains in the polyether compound except the main chain, wherein the main chain refers to the carbon chain containing the largest number of carbon atoms.
[0059] The present invention does not limit the specific carbon atom content in the branch chain, and the carbon atom content in each branch chain may be the same or different.
[0060] When the number of side chains of the polyether compound in the polyether wetting agent is within the above range, the surface tension of the polyether wetting agent can be within an appropriate range, and the diamond wire cutting fluid including the polyether wetting agent has more excellent cutting performance.
[0061] On the other hand, the present invention provides a method for preparing the diamond wire cutting fluid as described above, comprising the following steps: mixing a block polyether lubricant, a polyether wetting agent, and a polyether leveling agent, then adding water and stirring for 3-4 hours, and aging for 1 hour to obtain the diamond wire cutting fluid.
[0062] In detail, a block polyether lubricant with a molecular weight of 2000-6000, a polyether wetting agent with a molecular weight of 100-1000, and a polyether leveling agent with a molecular weight not higher than 4000 are added to the reactor in sequence, the three are mixed evenly, and then ultrapure water is added and stirred for 3-4 hours. After adding water, the circulating pipeline pump is turned on, and the mixture is stirred while circulating for 1 hour. After aging for 1 hour, a diamond wire cutting liquid is obtained, in which the block polyether lubricant is 20-30 parts, the polyether wetting agent is 10-15 parts, and the polyether leveling agent is 1-5 parts by weight.
[0063] Furthermore, in a specific embodiment of the present invention, during mixing, the stirring speed is 1000-1500 rpm, and the stirring time is 30-60 min.
[0064] Specifically, a block polyether lubricant, a polyether wetting agent, and a polyether leveling agent are sequentially added into a reaction kettle, and then stirred at a stirring speed of 1000-1500 rpm for 30-60 minutes.
[0065] Specifically, the stirring speed includes but is not limited to 1000 rpm, 1100 rpm, 1200 rpm, 1300 rpm, 1400 rpm, 1500 rpm or a range between any two of them.
[0066] The stirring time includes but is not limited to 30 rpm, 32 rpm, 34 rpm, 36 rpm, 38 rpm, 40 rpm, 42 rpm, 44 rpm, 46 rpm, 48 rpm, 50 rpm or a range between any two of them.
[0067] When the above stirring parameters are selected, the mixing of various components can be better achieved, thereby improving the uniformity and stability of the diamond wire cutting fluid.
[0068] Another aspect of the present invention provides a silicon wafer cutting method, which uses the diamond wire cutting liquid as described above or the diamond wire cutting liquid prepared according to the preparation method as described above to cut the silicon wafer.
[0069] Since the silicon wafer cutting method provided by the present invention uses the diamond wire cutting liquid or the diamond wire cutting liquid prepared according to the preparation method to cut the silicon wafer, the generation of edge chipping can be effectively reduced during the silicon wafer cutting process.
[0070] The diamond wire cutting fluid provided by the present invention is introduced below through specific embodiments.
[0071] Example 1
[0072] The diamond wire cutting fluid provided in this embodiment is prepared by the following steps:
[0073] Add a block polyether lubricant BPE-1000 with a mass average molecular weight of 2000 and a surface tension of 40 mN / m, a polyether wetting agent polyoxyethylene octanoate with a mass average molecular weight of 100 and a surface tension of 30 mN / m, and a polyether leveling agent Surfony 104 with a mass average molecular weight of 400 and a surface tension of 25 mN / m to the reactor in sequence, stir for 60 min at 1000 rpm, then add ultrapure water and stir for 3 h, start the circulation pipeline pump after adding water, stir for 1 h while circulating, and age for 1 h to obtain a diamond wire cutting liquid;
[0074] Among them, the diamond wire cutting fluid provided in this embodiment contains 20 parts of block polyether lubricant, 15 parts of polyether wetting agent, and 5 parts of polyether leveling agent in terms of mass parts; the number of side chains of the polyether compound in the polyether wetting agent is 40%, and the mass ratio of ultrapure water to functional components is 5:2.
[0075] Example 2
[0076] The diamond wire cutting fluid provided in this embodiment is prepared by the following steps:
[0077] To the reactor, a block polyether lubricant PE-10400 with a mass average molecular weight of 6000 and a surface tension of 50 mN / m, a polyether wetting agent L31 with a mass average molecular weight of 1000 and a surface tension of 35 mN / m, and a polyether leveling agent Zonoyl FSO with a mass average molecular weight of 950 and a surface tension of 26 mN / m were added in sequence, and stirred at 1500 rpm for 30 min, and then ultrapure water was added and stirred for 4 h. After adding water, a circulating pipeline pump was turned on, and the mixture was stirred for 1 h while circulating, and aged for 1 h to obtain a diamond wire cutting liquid;
[0078] The diamond wire cutting fluid provided in this embodiment comprises 30 parts by mass of segmented polyether lubricant, 10 parts by mass of polyether wetting agent and 1 part by mass of polyether leveling agent; the number of side chains of the polyether compound in the polyether wetting agent is 50%.
[0079] Example 3
[0080] The diamond wire cutting fluid provided in this embodiment is prepared by the following steps:
[0081] Add a block polyether lubricant PE6400 with a mass average molecular weight of 4000 and a surface tension of 45 mN / m, a polyether wetting agent XP90 with a mass average molecular weight of 500 and a surface tension of 33 mN / m, and a polyether leveling agent EFKA-3580 with a mass average molecular weight of 800 and a surface tension of 24 mN / m to the reactor in sequence, stir for 50 min at 1300 rpm, then add ultrapure water and stir for 3.5 h, start the circulation pipeline pump after adding water, stir for 1 h while circulating, and age for 1 h to obtain a diamond wire cutting liquid;
[0082] The diamond wire cutting fluid provided in this embodiment comprises 25 parts by weight of segmented polyether lubricant, 12 parts by weight of polyether wetting agent, and 3 parts by weight of polyether leveling agent; the number of side chains of the polyether compound in the polyether wetting agent is 60%.
[0083] Example 4
[0084] The preparation method of the diamond wire cutting fluid provided in this embodiment is basically the same as that in embodiment 3, except that:
[0085] In terms of parts by mass, the block polyether lubricant is 22 parts, the polyether wetting agent is 10 parts, and the polyether leveling agent is 2 parts.
[0086] Example 5
[0087] The preparation method of the diamond wire cutting fluid provided in this embodiment is basically the same as that in embodiment 3, except that:
[0088] The mass average molecular weight of the block polyether lubricant is 4500 and the surface tension is 47 mN / m.
[0089] Example 6
[0090] The preparation method of the diamond wire cutting fluid provided in this embodiment is basically the same as that in embodiment 3, except that:
[0091] The mass average molecular weight of the polyether wetting agent is 1000 and the surface tension is 34 mN / m.
[0092] Example 7
[0093] The preparation method of the diamond wire cutting fluid provided in this embodiment is basically the same as that in embodiment 3, except that:
[0094] The mass average molecular weight of the polyether wetting agent is 600, and the surface tension is 36 mN / m. The mass average molecular weight of the polyether leveling agent is 950, and the surface tension is 29 mN / m.
[0095] Example 8
[0096] The preparation method of the diamond wire cutting fluid provided in this embodiment is basically the same as that in embodiment 3, except that:
[0097] The block polyether lubricant is a regular block polyether with a mass average molecular weight of 4000, specifically PE6400.
[0098] Example 9
[0099] The preparation method of the diamond wire cutting fluid provided in this embodiment is basically the same as that in embodiment 3, except that:
[0100] The number of side chains of the polyether compound in the polyether wetting agent is 10%, the mass average molecular weight is 800, and the surface tension is 34 mN / m.
[0101] Comparative Example 1
[0102] The preparation method of the diamond wire cutting fluid provided in this comparative example is basically the same as that in Example 3, except that:
[0103] In terms of parts by mass, the block polyether lubricant is 18 parts, the polyether wetting agent is 20 parts, and the polyether leveling agent is 8 parts.
[0104] Comparative Example 2
[0105] The preparation method of the diamond wire cutting liquid provided in this comparative example comprises the following steps:
[0106] To the reactor, a block polyether lubricant BPE-1500 with a mass average molecular weight of 1500 and a surface tension of 41 mN / m, a polyether wetting agent L42 with a mass average molecular weight of 1500 and a surface tension of 38 mN / m, and a polyether leveling agent Dow Corning DC-65 with a mass average molecular weight of 5000 and a surface tension of 30 mN / m were added in sequence, and stirred at 1300 rpm for 50 min, and then ultrapure water was added and stirred for 3.5 h. After adding water, a circulating pipeline pump was turned on, and the mixture was stirred for 1 h while circulating, and aged for 1 h to obtain a diamond wire cutting fluid;
[0107] The diamond wire cutting fluid provided in this comparative example comprises 25 parts by weight of segmented polyether lubricant, 12 parts by weight of polyether wetting agent, and 3 parts by weight of polyether leveling agent; the number of side chains of the polyether compound in the polyether wetting agent is 40%.
[0108] Comparative Example 3
[0109] The preparation method of the diamond wire cutting fluid provided in this comparative example is basically the same as that in Example 3, except that:
[0110] The polyether leveling agent was replaced by polyacrylate with a mass average molecular weight of 2000 and a surface tension of 50 mN / m.
[0111] Comparative Example 4
[0112] The preparation method of the diamond wire cutting fluid provided in this comparative example is basically the same as that in Example 3, except that:
[0113] Among them, the mass ratio of functional components to ultrapure water is 1:4.
[0114] Test Case
[0115] 1. The diamond wire cutting fluids provided in all embodiments and comparative examples were subjected to a dynamic surface tension test, specifically comprising the following steps:
[0116] First calibrate with 25℃ ultrapure water Dynamic surface tension tester, dynamic surface tension of ultrapure water at 25°C is 72.0 mN / m. After calibration, the dynamic surface tension test range is set to 100ms to 1000ms. The cutting fluid prepared according to implementation method 10 is sampled and diluted to 0.5% with pure water. The dynamic surface tension of 1000ms is measured at 25°C using a dynamic surface tension meter.
[0117] The dynamic surface tension test results are shown in Table 1.
[0118] 2. Using the diamond wire cutting fluid provided in all the embodiments and comparative examples to perform a cutting test on a silicon wafer, specifically comprising the following steps:
[0119] Under the conditions of the same steel wire, wire transfer process, silicon wafer specifications, machine model, silicon rod glue, and cutting fluid addition amount, replace the experimental cutting fluid with different ratios and carry out silicon wafer cutting.
[0120] The statistics of silicon wafer cutting are shown in Table 1. Figure 1 This is a picture of a silicon wafer cut by the diamond wire cutting fluid provided in Example 3 of the present invention. Figure 2 This is a picture of a silicon wafer cut by the diamond wire cutting fluid provided in Comparative Example 3 of the present invention.
[0121] Table 1
[0122]
[0123]
[0124] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A diamond wire cutting fluid, It is characterized in that Includes functional components and water; The functional components include 20-30 parts by weight of block polyether lubricant, 10-15 parts of polyether wetting agent, and 1-5 parts of polyether leveling agent; The mass average molecular weight of the block polyether lubricant is 2000-6000, the mass average molecular weight of the polyether wetting agent is 100-1000, and the mass average molecular weight of the polyether leveling agent is not higher than 4000; The polyether leveling agent includes at least one of fluorine-modified polyether, silicon-modified polyether and bridge structure polyether; The mass ratio of the functional component to the water is 2:
5.
2. The diamond wire cutting fluid according to claim 1, It is characterized in that The functional components include 24-26 parts by weight of block polyether lubricant, 12-14 parts by weight of polyether wetting agent, and 3-4 parts by weight of polyether leveling agent.
3. The diamond wire cutting fluid according to claim 1 or 2, It is characterized in that The mass average molecular weight of the block polyether lubricant is 2000-4000.
4. The diamond wire cutting fluid according to any one of claims 1 to 3, It is characterized in that The mass average molecular weight of the polyether wetting agent is 300-800.
5. The diamond wire cutting fluid according to any one of claims 1 to 4, It is characterized in that The surface tension of the block polyether lubricant is 40-50 mN / m; And / or, the surface tension of the polyether wetting agent is 30-35 mN / m; And / or, the surface tension of the polyether leveling agent is not higher than 25 mN / m.
6. The diamond wire cutting fluid according to any one of claims 1 to 5, It is characterized in that The block polyether lubricant is a random block polyether lubricant.
7. The diamond wire cutting fluid according to any one of claims 1 to 6, It is characterized in that The molar amount of branched chains of the polyether compound in the polyether wetting agent is greater than 40%.
8. A method for preparing the diamond wire cutting fluid according to any one of claims 1 to 7, It is characterized in that The following steps are involved: The block polyether lubricant, the polyether wetting agent and the polyether leveling agent are mixed, and then water is added and stirred for 3-4 hours, and aged for 1 hour to obtain the diamond wire cutting liquid.
9. The preparation method according to claim 8, It is characterized in that During the mixing, the stirring speed is 1000-1500 rpm and the stirring time is 30-60 min.
10. A method for cutting a silicon wafer, It is characterized in that Silicon wafers are cut using the diamond wire cutting liquid described in any one of claims 1 to 7 or the diamond wire cutting liquid prepared by the preparation method described in claim 8 or 9.