High-efficiency carbon deposit cleaning agent for engine and preparation method of high-efficiency carbon deposit cleaning agent

By using a combination of modified composite molecular sieve catalyst and amphoteric polymerization dispersant, the existing carbon deposit cleaning methods are solved, and the problem of low efficiency and possible damage to the engine is achieved, and the efficient and non-corrosive carbon deposit cleaning effect is achieved, which significantly reduces the internal of the engine The formation of carbon deposits.

CN119020108APending Publication Date: 2024-11-26WUHAN WARD HUITONG AUTO SERVICE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411115145.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing carbon deposit cleaning methods are inefficient and may damage engine parts. The removal rate of existing carbon deposit removal agents is only up to 77.3%, and the effect still needs to be improved.

Method used

A combination of sodium tripolyphosphate, sodium metasilicate, sodium carbonate, composite surfactant, carboxyethylthiosuccinic acid, alkyl phosphate, modified composite molecular sieve catalyst and amphoteric polymerization dispersant was prepared. The efficient carbon deposit cleaning agent improves the catalytic performance and dispersion through the joint action of the modified composite molecular sieve catalyst and amphoteric polymerization dispersant, and achieves efficient carbon deposit removal.

Benefits of technology

It has achieved efficient removal of carbon deposits in the automobile engine while significantly reducing the formation of carbon deposits inside the engine, and the cleaning rate is efficient and non-corrosive.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the technical field of automobile cleaning, and particularly relates to an efficient carbon deposit cleaning agent for an engine and a preparation method of the carbon deposit cleaning agent. The carbon deposit cleaning agent comprises the following components in parts by mass: 10-30 parts of sodium tripolyphosphate, 30-45 parts of sodium metasilicate, 20-30 parts of sodium carbonate, 1-3 parts of a composite surfactant, 2-5 parts of carboxyethyl thiosuccinic acid, 2-4 parts of alkyl phosphate, 0.1-1 part of a modified composite molecular sieve catalyst, 1-3 parts of isooctyl alcohol and 0.5-1.5 parts of an amphoteric polymeric dispersant, the composite surface active agent comprises a nonionic surface active agent and a cationic surface active agent. The carbon deposit cleaning agent disclosed by the invention is simple in preparation process and use method, free of corrosivity, and capable of remarkably reducing formation of carbon deposits in an engine while efficiently removing carbon deposits in the automobile engine.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of automobile cleaning, and in particular relates to a high-efficiency carbon deposit cleaning agent for an engine and a preparation method thereof. Background Art

[0002] Carbon deposits are a kind of scorched substance produced by unsaturated olefins and colloids in fuel at high temperatures during the operation of automobile engines. The composition of carbon deposits is relatively complex, mainly containing hydroxy acids, asphaltene, oil coke and ash. After the formation of carbon deposits, it will seriously affect the normal operation of the engine. It can gather in various parts of the engine, such as the intake and exhaust system, combustion chamber, fuel injector, etc., resulting in a decrease in motor vehicle power, local overheating of the piston, increased fuel consumption, and even damage to the piston in severe cases. Therefore, it is very necessary to regularly clean the carbon deposits formed inside the automobile engine.

[0003] At present, the cleaning methods of carbon deposits mainly include mechanical methods and chemical methods. The mechanical method is to use mechanical tools to clean carbon deposits. This method is inefficient, some parts are not easy to clean, and scratches are easily formed; while the chemical method is to use acid and alkali reagents for cleaning, but it may cause serious damage to engine parts. Therefore, researchers are actively looking for a suitable solution to achieve a higher carbon deposit removal effect without damaging the engine. Patent CN 112143569A discloses a car engine carbon deposit cleaner and its use method. The carbon deposit cleaner includes oil spill dispersant, high temperature resistant aromatic silicone oil, organic water softener, dodecylphenol sulfonic acid isopropylamine salt, nonylphenol polyoxyethylene ether, red blood salt solution, etc. The car engine carbon deposit cleaner in the invention can remove carbon deposits in the engine to a certain extent, and can have a good cleaning effect on the parts with serious carbon deposit accumulation. However, the carbon deposit removal rate of the embodiment of this invention is only up to 77.3%, and the effect of the carbon deposit remover still needs to be improved.

[0004] Therefore, based on the problems existing in the prior art, it is of great practical significance to invent an efficient scavenger for cleaning carbon deposits in automobile engines. Summary of the invention

[0005] In view of the deficiencies in the prior art, the present invention provides an efficient, engine carbon deposit cleaning agent and a preparation method thereof. The preparation process and use method of the carbon deposit cleaning agent are simple and non-corrosive. While efficiently removing carbon deposits from automobile engines, it can also significantly reduce the formation of carbon deposits inside the engine.

[0006] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0007] The first aspect of the present invention provides a high-efficiency carbon deposit cleaning agent for an engine, which comprises the following components in parts by mass:

[0008] 10-30 parts of sodium tripolyphosphate, 30-45 parts of sodium metasilicate, 20-30 parts of sodium carbonate, 1-3 parts of composite surfactant, 2-5 parts of carboxyethyl thiosuccinic acid, 2-4 parts of alkyl phosphate, 0.1-1 parts of modified composite molecular sieve catalyst, 1-3 parts of isooctyl alcohol, and 0.5-1.5 parts of amphoteric polymer dispersant;

[0009] The complex surfactant includes a nonionic surfactant and a cationic surfactant.

[0010] Preferably, the nonionic surfactant is a polyoxyethylene ether surfactant; and the cationic surfactant is hexadecyltrimethyl quaternary ammonium bromide or octadecyldimethylbenzyl quaternary ammonium chloride.

[0011] In some embodiments, the preparation steps of the modified composite molecular sieve catalyst are:

[0012] (1) calcining molecular sieves HZSM-5 and SBA-15 at 550-560° C. for 150-180 h respectively, and mixing the calcined HZSM-5 and SBA-15 in a mass ratio of 1:(3-5) to obtain a composite molecular sieve;

[0013] (2) adding the composite molecular sieve of step (1) to a glucose aqueous solution, stirring at 40-50° C. for 18-24 h, crystallizing at 165° C.-185° C. for 12-16 h, naturally cooling, washing with water until neutral, drying, and calcining at 550-560° C. for 3-4 h to obtain a pretreated composite molecular sieve 1;

[0014] (3) ultrasonically dispersing the pretreated composite molecular sieve 1 of step (2) in a 3-aminopropyltriethoxysilane-toluene solution, reflux for 10-12 hours at 110-120° C. under the protection of an inert gas, centrifuging, washing, and drying to obtain a pretreated composite molecular sieve 2;

[0015] (4) immersing the pretreated composite molecular sieve 2 in step (3) in a nickel salt aqueous solution, stirring at 60-70° C. for 20-30 min, standing at room temperature for 20-24 h, drying, and calcining at 550-560° C. for 5-6 h to obtain a Ni-composite molecular sieve precursor;

[0016] (5) The Ni-composite molecular sieve precursor in step (4) is immersed in a lanthanum salt aqueous solution, stirred at 60-70° C. for 20-30 min, allowed to stand at room temperature for 20-24 h, dried, and calcined at 550-560° C. for 5-6 h to obtain a modified composite molecular sieve catalyst.

[0017] In some embodiments, the mass ratio of the composite molecular sieve to the glucose aqueous solution in step (2) is 1:(35-45); the concentration of the glucose aqueous solution is 3-7wt%.

[0018] Preferably, in step (2), the mass ratio of the composite molecular sieve to the glucose aqueous solution is 1:40; and the concentration of the glucose aqueous solution is 5 wt%.

[0019] In some embodiments, the ratio of the pretreated composite molecular sieve 1 to the 3-aminopropyltriethoxysilane-toluene solution in step (3) is 1 g:(110-120) mL; the volume ratio of 3-aminopropyltriethoxysilane to toluene in the 3-aminopropyltriethoxysilane-toluene solution is 25:(1-5).

[0020] Preferably, in the step (3), the ratio of the pretreated composite molecular sieve 1 to the 3-aminopropyltriethoxysilane-toluene solution is 1 g:115 mL; the volume ratio of 3-aminopropyltriethoxysilane to toluene in the 3-aminopropyltriethoxysilane-toluene solution is 25:2.5.

[0021] In some embodiments, the loading amounts of nickel salt and lanthanum salt in the modified composite molecular sieve catalyst are 10-12 wt% and 1-3 wt%, respectively.

[0022] Preferably, the loading amounts of nickel salt and lanthanum salt in the modified composite molecular sieve catalyst are 11 wt% and 2 wt%, respectively.

[0023] In some embodiments, the preparation steps of the amphoteric polymeric dispersant are:

[0024] Take allyl polyethylene glycol and add it into distilled water and stir evenly. At 70-80° C., add dropwise an aqueous solution containing acrylic acid and methacryloyloxyethyltrimethylammonium chloride, and then add dropwise an initiator solution. After the addition is completed, keep warm for 2-3 hours, adjust the pH to 6-7, and obtain an amphoteric polymer dispersant.

[0025] In some embodiments, the Mn of the allyl polyethylene glycol is 2000-2400.

[0026] In some embodiments, the molar ratio of allyl polyethylene glycol, acrylic acid and methacryloyloxyethyltrimethylammonium chloride is 1:(2-4):(0.5-2).

[0027] Preferably, the molar ratio of allyl polyethylene glycol, acrylic acid and methacryloyloxyethyltrimethylammonium chloride in the amphoteric polymer dispersant is 1:3:1.

[0028] In some embodiments, the Mn of the amphoteric polymeric dispersant is (1-1.2)×10 4.

[0029] Preferably, the Mn of the amphoteric polymer dispersant is (1.05-1.1)×10 4 .

[0030] The present invention prepares a carbon deposit remover by mixing sodium tripolyphosphate, sodium metasilicate, sodium carbonate, a composite surfactant, carboxyethyl thiosuccinic acid, an alkyl phosphate, a modified composite molecular sieve catalyst, isooctyl alcohol and an amphoteric polymer dispersant in a certain ratio. The components can work together to achieve a good carbon deposit removal effect on automobile engine carbon deposits and other parts, and can also significantly inhibit the formation of carbon deposits inside the engine.

[0031] First, the present invention prepares a composite molecular sieve catalyst, HZSM-5 and SBA-15 are mixed according to a specific ratio, and then processed by glucose and 3-aminopropyltriethoxysilane in sequence, and then nickel salt and lanthanum salt are loaded to improve the comprehensive performance of the catalyst. The applicant finds that the composite molecular sieve is hydrothermally modified by glucose aqueous solution, and glucose can produce levulinic acid during the treatment process, which plays a role of slow acid treatment on the composite molecular sieve, so that the catalyst skeleton structure is intact, and dealumination will also occur, so that the average pore size inside the catalyst is increased, and more mesoporous structures appear, which is conducive to the diffusion of reactants and products, and can slow down the accumulation rate of carbon deposition. Then, the composite molecular sieve treated with glucose is modified using 3-aminopropyltriethoxysilane with an amino functional group, and the amino functional group is grafted on the surface of the molecular sieve, which can chelate with nickel ions and lanthanum ions, enhance the binding force of the molecular sieve catalyst with them, form a stable coordination compound, and improve the catalytic performance of the modified composite molecular sieve catalyst.

[0032] Secondly, since the carbon deposit cleaning agent of the present invention is used after being dissolved in water, and the modified composite molecular sieve catalyst has poor dispersibility in water, the present invention synthesizes an amphoteric polymer dispersant, which is used together with the modified composite molecular sieve catalyst to improve its water dispersibility and stability. The present invention adopts an aqueous solution free radical polymerization method, and introduces anionic groups (carboxyl groups) and cationic groups (quaternary ammonium salts) on allyl polyethylene glycol at the same time. The electrostatic interaction between anions and cations can enhance the adsorption of the dispersant on the catalyst surface, and the polyether monomer on the dispersant can also provide a certain steric hindrance, which significantly improves the agglomeration problem of the modified composite molecular sieve catalyst.

[0033] The second aspect of the present invention provides a method for preparing an efficient carbon deposit cleaning agent for an engine, comprising the following preparation steps:

[0034] The modified composite molecular sieve catalyst is firstly mixed with the amphoteric polymer dispersant, and then mixed with sodium tripolyphosphate, sodium metasilicate, sodium carbonate, composite surfactant, carboxyethyl thiosuccinic acid, alkyl phosphate and isooctyl alcohol, and stirred evenly to obtain a carbon deposit cleaning agent.

[0035] Compared with the prior art, the present invention has the following beneficial effects:

[0036] 1. The present invention provides an efficient carbon deposit cleaning agent for engines. The preparation process and use method of the carbon deposit cleaning agent are simple and non-corrosive. While efficiently removing carbon deposits from automobile engines, it can also significantly reduce the formation of carbon deposits inside the engine.

[0037] 2. The present invention prepares a composite molecular sieve catalyst, wherein HZSM-5 and SBA-15 are mixed in a specific ratio, treated with a certain concentration of glucose and 3-aminopropyltriethoxysilane in turn, and then loaded with nickel salt and lanthanum salt, which significantly improves the catalytic and stability performance of the catalyst.

[0038] 3. The present invention synthesizes an amphoteric polymer dispersant, and the dispersant is used together with a modified composite molecular sieve catalyst to improve the dispersibility and stability of the catalyst in water. DETAILED DESCRIPTION

[0039] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0040] In order to better illustrate the specific implementation of the present invention, the following examples are further illustrated. The mass fractions described in the following examples can be grams, kilograms, tons or other mass units.

[0041] The initiator used in the present invention is ammonium persulfate; the alkyl phosphate used is dodecyl phosphate; the alkylphenol polyoxyethylene ether used is alkylphenol polyoxyethylene ether NP-12, purchased from Shandong Zibo Haijie Chemical Co., Ltd.; the Mn of the allyl polyethylene glycol used is 2400, purchased from Jiangsu Haian Petrochemical Plant.

[0042] Preparation Example 1

[0043] The preparation steps of the modified composite molecular sieve catalyst are:

[0044] (1) molecular sieves HZSM-5 and SBA-15 were calcined at 555°C for 165h respectively, and 10g of the calcined HZSM-5 and 40g of SBA-15 were mixed to obtain a composite molecular sieve;

[0045] (2) 5 g of the composite molecular sieve prepared in step (1) was added to 200 g of a 5 wt% glucose aqueous solution, stirred at 40° C. for 24 h, crystallized at 165° C. for 16 h, naturally cooled, washed with water until neutral, dried at 100° C. to constant weight, and calcined at 555° C. for 4 h to obtain a pretreated composite molecular sieve 1;

[0046] (3) 2 g of the pretreated composite molecular sieve 1 of step (2) was ultrasonically dispersed in 230 mL of 3-aminopropyltriethoxysilane-toluene solution (including 205 mL of toluene and 25 mL of 3-aminopropyltriethoxysilane), refluxed at 115° C. for 12 h under the protection of nitrogen, centrifuged, washed with water until neutral, and dried at 100° C. to constant weight to obtain a pretreated composite molecular sieve 2;

[0047] (4) 2 g of the pretreated composite molecular sieve 2 in step (3) was immersed in 3 mL of 73 mg / mL nickel nitric acid aqueous solution, stirred at 65 ° C for 30 min, allowed to stand at room temperature for 20 h, dried at 100 ° C to constant weight, and calcined at 555 ° C for 5 h to obtain a Ni-composite molecular sieve precursor;

[0048] (5) 2 g of the Ni-composite molecular sieve precursor in step (4) was immersed in 3 mL of 13.3 mg / mL lanthanum nitrate aqueous solution, stirred at 65 ° C for 30 min, allowed to stand at room temperature for 20 h, dried at 100 ° C to constant weight, and calcined at 555 ° C for 5 h to obtain a modified composite molecular sieve catalyst.

[0049] Preparation Example 2

[0050] The preparation steps of the modified composite molecular sieve catalyst are:

[0051] (1) molecular sieves HZSM-5 and SBA-15 were calcined at 555°C for 165h respectively, and 10g of the calcined HZSM-5 and 40g of SBA-15 were mixed to obtain a composite molecular sieve;

[0052] (2) 2 g of the composite molecular sieve of step (1) was ultrasonically dispersed in 230 mL of 3-aminopropyltriethoxysilane-toluene solution (including 205 mL of toluene and 25 mL of 3-aminopropyltriethoxysilane), refluxed at 115° C. for 12 h under the protection of nitrogen, centrifuged, washed with water until neutral, and dried at 100° C. to constant weight to obtain a pretreated composite molecular sieve 2;

[0053] (3) 2 g of the pretreated composite molecular sieve 2 in step (2) was immersed in 3 mL of 73 mg / mL nickel nitric acid aqueous solution, stirred at 65 ° C for 30 min, allowed to stand at room temperature for 20 h, dried at 100 ° C to constant weight, and calcined at 555 ° C for 5 h to obtain a Ni-composite molecular sieve precursor;

[0054] (4) 2 g of the Ni-composite molecular sieve precursor in step (3) was immersed in 3 mL of 13.3 mg / mL lanthanum nitrate aqueous solution, stirred at 65 ° C for 30 min, allowed to stand at room temperature for 20 h, dried at 100 ° C to constant weight, and calcined at 555 ° C for 5 h to obtain a modified composite molecular sieve catalyst.

[0055] Preparation Example 3

[0056] The preparation steps of the modified composite molecular sieve catalyst are:

[0057] (1) molecular sieves HZSM-5 and SBA-15 were calcined at 555°C for 165h respectively, and 10g of the calcined HZSM-5 and 40g of SBA-15 were mixed to obtain a composite molecular sieve;

[0058] (2) 5 g of the composite molecular sieve prepared in step (1) was added to 200 g of a 5 wt% glucose aqueous solution, stirred at 40° C. for 24 h, crystallized at 165° C. for 16 h, naturally cooled, washed with water until neutral, dried at 100° C. to constant weight, and calcined at 555° C. for 4 h to obtain a pretreated composite molecular sieve 1;

[0059] (3) 2 g of the pretreated composite molecular sieve 1 in step (2) was immersed in 3 mL of 73 mg / mL nickel nitric acid aqueous solution, stirred at 65 ° C for 30 min, allowed to stand at room temperature for 20 h, dried at 100 ° C to constant weight, and calcined at 555 ° C for 5 h to obtain a Ni-composite molecular sieve precursor;

[0060] (4) 2 g of the Ni-composite molecular sieve precursor in step (3) was immersed in 3 mL of 13.3 mg / mL lanthanum nitrate aqueous solution, stirred at 65 ° C for 30 min, allowed to stand at room temperature for 20 h, dried at 100 ° C to constant weight, and calcined at 555 ° C for 5 h to obtain a modified composite molecular sieve catalyst.

[0061] Preparation Example 4

[0062] The preparation steps of the modified composite molecular sieve catalyst are:

[0063] (1) molecular sieves HZSM-5 and SBA-15 were calcined at 555°C for 165h respectively, and 10g of the calcined HZSM-5 and 40g of SBA-15 were mixed to obtain a composite molecular sieve;

[0064] (2) 2 g of the composite molecular sieve prepared in step (1) was immersed in 3 mL of 73 mg / mL nickel nitric acid aqueous solution, stirred at 65 ° C for 30 min, allowed to stand at room temperature for 20 h, dried at 100 ° C to constant weight, and calcined at 555 ° C for 5 h to obtain a Ni-composite molecular sieve precursor;

[0065] (3) 2 g of the Ni-composite molecular sieve precursor in step (2) was immersed in 3 mL of 13.3 mg / mL lanthanum nitrate aqueous solution, stirred at 65 ° C for 30 min, allowed to stand at room temperature for 20 h, dried at 100 ° C to constant weight, and calcined at 555 ° C for 5 h to obtain a modified composite molecular sieve catalyst.

[0066] Preparation Example 5

[0067] The preparation steps of the modified molecular sieve catalyst are:

[0068] (1) calcining molecular sieve HZSM-5 at 555° C. for 165 h to obtain calcined molecular sieves;

[0069] (2) adding 5 g of the calcined molecular sieve obtained in step (1) to 200 g of a 5 wt% glucose aqueous solution, stirring at 40° C. for 24 h, crystallizing at 165° C. for 16 h, naturally cooling, washing with water until neutral, drying at 100° C. to constant weight, and calcining at 555° C. for 4 h to obtain pretreated molecular sieve 1;

[0070] (3) 2 g of the pretreated molecular sieve 1 of step (2) was ultrasonically dispersed in 230 mL of 3-aminopropyltriethoxysilane-toluene solution (including 205 mL of toluene and 25 mL of 3-aminopropyltriethoxysilane), refluxed at 115° C. for 12 h under the protection of nitrogen, centrifuged, washed with water until neutral, and dried at 100° C. to constant weight to obtain pretreated molecular sieve 2;

[0071] (4) 2 g of the pretreated molecular sieve 2 in step (3) was immersed in 3 mL of 73 mg / mL nickel nitric acid aqueous solution, stirred at 65 ° C for 30 min, allowed to stand at room temperature for 20 h, dried at 100 ° C to constant weight, and calcined at 555 ° C for 5 h to obtain a Ni-molecular sieve precursor;

[0072] (5) 2 g of the Ni-molecular sieve precursor in step (4) was immersed in 3 mL of 13.3 mg / mL lanthanum nitrate aqueous solution, stirred at 65 ° C for 30 min, allowed to stand at room temperature for 20 h, dried at 100 ° C to constant weight, and calcined at 555 ° C for 5 h to obtain a modified molecular sieve catalyst.

[0073] Preparation Example 6

[0074] The preparation steps of the modified molecular sieve catalyst are:

[0075] (1) calcining molecular sieve SBA-15 at 555° C. for 165 h to obtain a calcined molecular sieve;

[0076] (2) 5 g of the calcined molecular sieve of step (1) was added to 200 g of a 5 wt% glucose aqueous solution, stirred at 45° C. for 24 h, crystallized at 165° C. for 16 h, naturally cooled, washed with water until neutral, dried at 100° C. to constant weight, and calcined at 555° C. for 4 h to obtain pretreated molecular sieve 1;

[0077] (3) 2 g of the pretreated molecular sieve 1 of step (2) was ultrasonically dispersed in 230 mL of 3-aminopropyltriethoxysilane-toluene solution (including 205 mL of toluene and 25 mL of 3-aminopropyltriethoxysilane), refluxed at 115° C. for 12 h under the protection of nitrogen, centrifuged, washed with water until neutral, and dried at 100° C. to constant weight to obtain pretreated molecular sieve 2;

[0078] (4) 2 g of the pretreated molecular sieve 2 in step (3) was immersed in 3 mL of 73 mg / mL nickel nitric acid aqueous solution, stirred at 65 ° C for 30 min, allowed to stand at room temperature for 20 h, dried at 100 ° C to constant weight, and calcined at 555 ° C for 5 h to obtain a Ni-molecular sieve precursor;

[0079] (5) 2 g of the Ni-molecular sieve precursor in step (4) was immersed in 3 mL of 13.3 mg / mL lanthanum nitrate aqueous solution, stirred at 65 ° C for 30 min, allowed to stand at room temperature for 20 h, dried at 100 ° C to constant weight, and calcined at 555 ° C for 5 h to obtain a modified molecular sieve catalyst.

[0080] Preparation Example 7

[0081] The preparation steps of the amphoteric polymeric dispersant are:

[0082] Take 0.1 mol of allyl polyethylene glycol and add it into 500 mL of distilled water and stir evenly. At 75°C, add 400 mL of an aqueous solution containing 0.3 mol of acrylic acid and 0.1 mol of methacryloyloxyethyltrimethylammonium chloride at a uniform rate within 2 h. Then, add 100 mL of 0.03 mol / L initiator solution at a uniform rate within 2 h. After the addition, keep warm at 75°C for 2.5 h, adjust the pH to 6.5, and obtain an amphoteric polymer dispersant.

[0083] Preparation Example 8

[0084] The preparation steps of the amphoteric polymeric dispersant are:

[0085] Take 0.1 mol of allyl polyethylene glycol and add it into 500 mL of distilled water and stir evenly. At 75°C, add 400 mL of an aqueous solution containing 0.3 mol of acrylic acid and 0.3 mol of methacryloyloxyethyltrimethylammonium chloride at a uniform rate within 2 h. Then, add 100 mL of 0.03 mol / L initiator solution at a uniform rate within 2 h. After the addition, keep warm at 75°C for 2.5 h, adjust the pH to 6.5, and obtain an amphoteric polymer dispersant.

[0086] Preparation Example 9

[0087] The preparation steps of the amphoteric polymeric dispersant are:

[0088] Take 0.1 mol of allyl polyethylene glycol and add it into 500 mL of distilled water and stir evenly. At 75°C, add 400 mL of an aqueous solution containing 0.45 mol of acrylic acid and 0.1 mol of methacryloyloxyethyltrimethylammonium chloride at a uniform rate within 2 h. Then, add 100 mL of 0.03 mol / L initiator solution at a uniform rate within 2 h. After the addition, keep warm at 75°C for 2.5 h, adjust the pH to 6.5, and obtain an amphoteric polymer dispersant.

[0089] Preparation Example 10

[0090] The preparation steps of the amphoteric polymeric dispersant are the same as those in Preparation Example 1, except that the Mn of the allyl polyethylene glycol used is 1000.

[0091] Example 1

[0092] A method for preparing an efficient carbon deposit cleaning agent for an engine comprises the following preparation steps:

[0093] First, mix 1g of the modified composite molecular sieve catalyst with 5g of the amphoteric polymer dispersant, and then mix with 100g of sodium tripolyphosphate, 300g of sodium metasilicate, 200g of sodium carbonate, 10g of a composite surfactant, 20g of carboxyethyl thiosuccinic acid, 20g of alkyl phosphate and 10g of isooctyl alcohol, stir evenly to obtain a carbon deposit cleaning agent.

[0094] The modified composite molecular sieve catalyst used is obtained from Preparation Example 1; the amphoteric polymer dispersant used is obtained from Preparation Example 7; and the composite surfactant used is composed of alkylphenol polyoxyethylene ether NP-12 and hexadecyltrimethylammonium chloride in a mass ratio of 1:1.

[0095] Example 2

[0096] A method for preparing an efficient carbon deposit cleaning agent for an engine comprises the following preparation steps:

[0097] First, 10g of the modified composite molecular sieve catalyst is evenly mixed with 15g of an amphoteric polymer dispersant, and then mixed with 200g of sodium tripolyphosphate, 400g of sodium metasilicate, 250g of sodium carbonate, 30g of a composite surfactant, 50g of carboxyethyl thiosuccinic acid, 40g of alkyl phosphate and 30g of isooctyl alcohol, and stirred evenly to obtain a carbon deposit cleaning agent.

[0098] The modified composite molecular sieve catalyst used is obtained from Preparation Example 1; the amphoteric polymer dispersant used is obtained from Preparation Example 7; and the composite surfactant used is composed of alkylphenol polyoxyethylene ether NP-12 and hexadecyltrimethylammonium chloride in a mass ratio of 1:1.

[0099] Example 3

[0100] A method for preparing an efficient carbon deposit cleaning agent for an engine comprises the following preparation steps:

[0101] First, mix 5g of the modified composite molecular sieve catalyst with 10g of the amphoteric polymer dispersant, and then mix with 300g of sodium tripolyphosphate, 450g of sodium metasilicate, 300g of sodium carbonate, 20g of composite surfactant, 40g of carboxyethyl thiosuccinic acid, 30g of alkyl phosphate and 20g of isooctyl alcohol, stir evenly to obtain a carbon deposit cleaning agent.

[0102] The modified composite molecular sieve catalyst used is obtained from Preparation Example 1; the amphoteric polymer dispersant used is obtained from Preparation Example 7; and the composite surfactant used is composed of alkylphenol polyoxyethylene ether NP-12 and hexadecyltrimethylammonium chloride in a mass ratio of 1:1.

[0103] Example 4

[0104] A method for preparing an efficient carbon deposit cleaning agent for an engine, wherein the specific implementation method is the same as that of Example 3, except that the modified composite molecular sieve catalyst used is obtained from Preparation Example 2.

[0105] Example 5

[0106] A method for preparing an efficient carbon deposit cleaning agent for an engine, wherein the specific implementation method is the same as that of Example 3, except that the modified composite molecular sieve catalyst used is obtained from Preparation Example 3.

[0107] Example 6

[0108] A method for preparing an efficient carbon deposit cleaning agent for an engine, wherein the specific implementation method is the same as that of Example 3, except that the modified composite molecular sieve catalyst used is obtained from Preparation Example 4.

[0109] Comparative Example 1

[0110] A method for preparing a highly efficient carbon deposit cleaning agent for an engine, wherein the specific implementation method is the same as that of Example 3, except that the modified molecular sieve catalyst of equal mass in Preparation Example 5 is used instead of the modified composite molecular sieve catalyst.

[0111] Comparative Example 2

[0112] A method for preparing a highly efficient carbon deposit cleaning agent for an engine, wherein the specific implementation method is the same as that of Example 3, except that the modified molecular sieve catalyst of equal mass in Preparation Example 6 is used instead of the modified composite molecular sieve catalyst.

[0113] Comparative Example 3

[0114] A method for preparing a highly efficient carbon deposit cleaning agent for an engine, wherein the specific implementation method is the same as that of Example 3, except that no modified composite molecular sieve catalyst is added.

[0115] Example 7

[0116] A method for preparing a highly efficient carbon deposit cleaning agent for an engine, wherein the specific implementation method is the same as that of Example 3, except that the amphoteric polymer dispersant used is obtained from Preparation Example 8.

[0117] Example 8

[0118] A method for preparing a highly efficient carbon deposit cleaning agent for an engine, wherein the specific implementation method is the same as that of Example 3, except that the amphoteric polymer dispersant used is obtained from Preparation Example 9.

[0119] Example 10

[0120] A method for preparing a highly efficient carbon deposit cleaning agent for an engine, the specific implementation method is the same as that of Example 3, except that the amphoteric polymer dispersant used is obtained from Preparation Example 10.

[0121] Comparative Example 4

[0122] A method for preparing a highly efficient carbon deposit cleaning agent for an engine, wherein the specific implementation method is the same as that of Example 3, except that no amphoteric polymer dispersant is added.

[0123] Performance test of carbon deposit cleaning agent

[0124] 1. Cleaning rate test

[0125] The carbon deposit cleaning agents prepared in the examples and comparative examples were mixed with pure water to prepare carbon deposit cleaning solutions with a concentration of 50 g / L, and a 50 g / L NaOH solution was used as the carbon deposit cleaning solution of the control group to conduct a cleaning rate test.

[0126] Preparation of aluminum alloy test pieces after carbon deposits: refer to the literature "Design and optimization of powdered carbon deposit cleaning agent formula";

[0127] Cleaning of aluminum alloy specimens with attached carbon deposits: first soak the aluminum alloy specimens with attached carbon deposits in anhydrous ethanol for 20 minutes, and then dry them in the air; then put the aluminum alloy specimens into 50g / L carbon deposit cleaning liquid / NaOH solution, ultrasonically treat them at 20kHz and 45°C for 30 minutes, clean the aluminum alloy specimens with ultrapure water for 5 times, and then clean them with anhydrous ethanol for 3 times, and dry them in the air to complete the cleaning.

[0128] The effect of the carbon deposit cleaning agent prepared in the embodiment and preparation example of the present invention was tested by weight method: the dry aluminum alloy test piece before cleaning and after carbon deposit was attached was weighed as W1, and the aluminum alloy test piece after cleaning and drying was weighed as W2, and the carbon deposit cleaning rate was calculated according to the following formula:

[0129] Cleaning rate (%) = [1-(W2-W0) / (W1-W0)] × 100%,

[0130] Where: W0 is the original mass of the aluminum alloy test piece without carbon deposits (g); W1 is the mass of the aluminum alloy test piece after carbon deposits (g); W2 is the mass of the aluminum alloy test piece after cleaning (g). Specific test data are shown in Table 1.

[0131] Table 1

[0132] serial number Cleaning rate (%) Surface corrosion of aluminum alloy test piece Example 1 85.5 The surface is smooth, exuding metallic luster, and is not corroded Example 2 86.7 The surface is smooth, exuding metallic luster, and is not corroded Example 3 88.3 The surface is smooth, exuding metallic luster, and is not corroded Example 4 84.2 The surface is smooth, exuding metallic luster, and is not corroded Example 5 84.0 The surface is smooth, exuding metallic luster, and is not corroded Example 6 84.8 The surface is smooth, exuding metallic luster, and is not corroded Example 7 83.9 The surface is smooth, exuding metallic luster, and is not corroded Example 8 83.8 The surface is smooth, exuding metallic luster, and is not corroded Example 9 82.6 The surface is smooth, exuding metallic luster, and is not corroded Example 10 83.2 The surface is smooth, exuding metallic luster, and is not corroded Comparative Example 1 81.4 The surface is smooth, exuding metallic luster, and is not corroded Comparative Example 2 80.9 The surface is smooth, exuding metallic luster, and is not corroded Comparative Example 3 76.5 The surface is smooth, exuding metallic luster, and is not corroded Comparative Example 4 75.2 The surface is smooth, exuding metallic luster, and is not corroded Control group 99.8 The surface is smooth, the metallic luster is exposed, and it is severely corroded

[0133] As can be seen from Table 1, although the carbon deposit cleaning agents prepared in Examples 1-3 have a less carbon deposit removal effect on the aluminum alloy test piece after carbon deposits are attached than the NaOH solution, they have no corrosive effect on the aluminum alloy test piece, and the cleaning rate is also relatively high. Compared with Example 3, in Examples 4-10, due to the change in the preparation process of the modified composite molecular sieve catalyst and the amphoteric polymer dispersant used, the catalytic effect of the modified composite molecular sieve catalyst is weakened, or the cleaning agent components are unevenly dispersed, affecting the function of the effective components, resulting in a decrease in the removal efficiency of the prepared carbon deposit cleaning agent to varying degrees. The catalytic effect of the modified molecular sieve catalyst used in Comparative Examples 1 and 2 is weaker than that of the modified composite molecular sieve catalyst, which reduces the removal efficiency of the carbon deposit cleaning agent; in Comparative Example 3, no modified composite molecular sieve catalyst is added, so that the carbon deposit cleaning agent does not have the effect of catalyzing the cracking of carbon deposits, and the cleaning effect is significantly reduced; in Comparative Example 4, no amphoteric polymer dispersant is added, and the dispersion effect of the components with cleaning effect in the system is poor, which also leads to a significant reduction in the cleaning effect.

[0134] 2. Carbon deposit inhibition test

[0135] Based on the data in Table 1, the carbon deposit remover of Example 3 and the carbon deposit removers of Comparative Examples 1-4 were selected to perform the following tests:

[0136] After the carbon deposit removers in Example 3 and Comparative Examples 1-4 were used to prepare a carbon deposit cleaning liquid with a concentration of 50 g / L with pure water to clean the Volkswagen imported Weilan 380TSI vehicles (completely cleaned), each vehicle was allowed to travel 25,000 km, and then the carbon deposits in the engines of each vehicle were checked using an automobile endoscope. The results showed that the vehicle using the carbon deposit remover in Example 3 had the least carbon deposits, and the vehicle using the carbon deposit remover in Comparative Example 3 had the most carbon deposits. This shows that the carbon deposit remover prepared in the present invention not only has a good carbon deposit removal effect, but also does not cause corrosion to the automobile engine, and can also better inhibit the occurrence of carbon deposits inside the automobile engine.

[0137] The above is only a preferred embodiment of the present invention and does not constitute any form of limitation to the present application. Although the present application is disclosed as above in the preferred embodiment, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases. However, any simple modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution.

Claims

1. A highly efficient carbon deposit cleaning agent for engines, characterized in that: According to the mass percentage, it includes the following components: 10-30 parts of sodium tripolyphosphate, 30-45 parts of sodium metasilicate, 20-30 parts of sodium carbonate, 1-3 parts of composite surfactant, 2-5 parts of carboxyethyl thiosuccinic acid, 2-4 parts of alkyl phosphate, 0.1-1 parts of modified composite molecular sieve catalyst, 1-3 parts of isooctyl alcohol, and 0.5-1.5 parts of amphoteric polymer dispersant; The complex surfactant includes a nonionic surfactant and a cationic surfactant.

2. The carbon deposit cleaning agent according to claim 1, characterized in that: The preparation steps of the modified composite molecular sieve catalyst are: (1) calcining molecular sieves HZSM-5 and SBA-15 at 550-560° C. for 150-180 h respectively, and mixing the calcined HZSM-5 and SBA-15 in a mass ratio of 1:(3-5) to obtain a composite molecular sieve; (2) adding the composite molecular sieve of step (1) to a glucose aqueous solution, stirring at 40-50° C. for 18-24 h, crystallizing at 165° C.-185° C. for 12-16 h, naturally cooling, washing with water until neutral, drying, and calcining at 550-560° C. for 3-4 h to obtain a pretreated composite molecular sieve 1; (3) ultrasonically dispersing the pretreated composite molecular sieve 1 of step (2) in a 3-aminopropyltriethoxysilane-toluene solution, reflux for 10-12 hours at 110-120° C. under the protection of an inert gas, centrifuging, washing, and drying to obtain a pretreated composite molecular sieve 2; (4) immersing the pretreated composite molecular sieve 2 in step (3) in a nickel salt aqueous solution, stirring at 60-70° C. for 20-30 min, standing at room temperature for 20-24 h, drying, and calcining at 550-560° C. for 5-6 h to obtain a Ni-composite molecular sieve precursor; (5) The Ni-composite molecular sieve precursor in step (4) is immersed in a lanthanum salt aqueous solution, stirred at 60-70° C. for 20-30 min, allowed to stand at room temperature for 20-24 h, dried, and calcined at 550-560° C. for 5-6 h to obtain a modified composite molecular sieve catalyst.

3. The carbon deposit cleaning agent according to claim 2, characterized in that: In the step (2), the mass ratio of the composite molecular sieve to the glucose aqueous solution is 1:(35-45); the concentration of the glucose aqueous solution is 3-7wt%.

4. The carbon deposit cleaning agent according to claim 2, characterized in that: In the step (3), the ratio of the pretreated composite molecular sieve 1 to the 3-aminopropyltriethoxysilane-toluene solution is 1 g:(110-120) mL; the volume ratio of 3-aminopropyltriethoxysilane to toluene in the 3-aminopropyltriethoxysilane-toluene solution is 25:(1-5).

5. The carbon deposit cleaning agent according to claim 2, characterized in that: The loading amounts of nickel salt and lanthanum salt in the modified composite molecular sieve catalyst are 10-12 wt% and 1-3 wt% respectively.

6. The carbon deposit cleaning agent according to claim 1, characterized in that: The preparation steps of the amphoteric polymer dispersant are: Take allyl polyethylene glycol and add it into distilled water and stir evenly. At 70-80° C., add dropwise an aqueous solution containing acrylic acid and methacryloyloxyethyltrimethylammonium chloride, and then add dropwise an initiator solution. After the addition is completed, keep warm for 2-3 hours, adjust the pH to 6-7, and obtain an amphoteric polymer dispersant.

7. The carbon deposit cleaning agent according to claim 6, characterized in that: The Mn of the allyl polyethylene glycol is 2000-2400.

8. The carbon deposit cleaning agent according to claim 7, characterized in that: The molar ratio of the allyl polyethylene glycol, acrylic acid and methacryloyloxyethyl trimethylammonium chloride is 1:(2-4):(0.5-2).

9. The carbon deposit cleaning agent according to claim 8, characterized in that: The Mn of the amphoteric polymer dispersant is (1-1.2)×10 4 .

10. A method for preparing the high-efficiency carbon deposit cleaning agent for engines as claimed in any one of claims 1 to 9, characterized in that: The method comprises the following preparation steps: The modified composite molecular sieve catalyst is firstly mixed with the amphoteric polymer dispersant, and then mixed with sodium tripolyphosphate, sodium metasilicate, sodium carbonate, composite surfactant, carboxyethyl thiosuccinic acid, alkyl phosphate and isooctyl alcohol, and stirred evenly to obtain a carbon deposit cleaning agent.