Refining slag system and application

By using a specific composition of refined slag system during steelmaking, the generation of high MgO content and pure MgO inclusions is solved, and the stability and cleanliness in the magnesium treatment process is achieved, and the high cleanliness and uniformity of the steel is achieved. , extends the life of the ladle and simplifies process operations.

CN119020554APending Publication Date: 2024-11-26UNIV OF SCI & TECH BEIJING
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410975402.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

During the steelmaking process, the existing magnesium treatment process has problems such as magnesium volatility, severe reaction, difficult process operation and unstable product quality, which makes it difficult to stably obtain high MgO content and pure MgO inclusions, which affects the cleanliness of the steel and performance.

Method used

The refined slag system is adopted, and the composition is CaO: 48.0-54.0%, Al2O3: 36.0-45.0%, MgO: 5.0-13.0%, SiO2 <3.0%. By adding refined slag during the steelmaking process, high MgO content and pure are controlled. MgO inclusions are appropriately adjusted in different processes, including converter, LF refining and RH vacuum treatment, ensuring uniform distribution of inclusions and cleanliness of the steel.

Benefits of technology

Stable obtaining fine high MgO content and pure MgO inclusions improves the cleanliness and uniformity of the steel, extends the service life of the ladle, simplifies process operations, avoids severe reactions and secondary oxidation of the steel, and improves the Product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020554A_ABST
    Figure CN119020554A_ABST
Patent Text Reader

Abstract

The invention relates to a refining slag system and application. The refining slag system comprises the following components in percentage by mass: 48.0 to 54.0 percent of CaO, 36.0 to 45.0 percent of Al2O3, 5.0 to 13.0 percent of MgO, less than 3.0 percent of SiO2 and the balance of inevitable impurities. According to the refining slag system, high MgO and pure MgO inclusions can be controlled to be generated in steel in the steelmaking process, meanwhile, molten steel can obtain very high cleanliness, and the oxygen content in the steel can be controlled to be 0.0010% or below.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of steelmaking, and in particular relates to a refined slag system and application thereof. Background Art

[0002] In recent years, the demand for high-quality steel has greatly increased, and users have increasingly stringent requirements for steel performance. Improving steel quality is an urgent problem for major steel companies. After deoxidation, a large amount of Al2O3 inclusions will be generated in the primary steelmaking of aluminum-killed steel converters or electric furnaces. Such inclusions tend to gather on the inner wall of the nozzle to form nodules, which seriously affect the castability of the molten steel. In addition, Al2O3 inclusions tend to gather in the molten steel to form large-sized clustered inclusions, which seriously affect the performance of the steel.

[0003] In order to improve the impact of Al2O3 inclusions on production and steel performance, inclusion modification technology has been used by major steel companies. Magnesium treatment technology is currently one of the effective means to modify Al2O3 inclusions. It can modify clustered Al2O3 inclusions into fine high MgO content and pure MgO inclusions. Such inclusions are not easy to aggregate in steel and are dispersed, which is beneficial to improve the cleanliness of molten steel. Compared with liquid CaO-Al2O3, controlling the inclusions in steel to high MgO content and pure MgO inclusions can effectively avoid the generation of large Ds-type inclusions. From the perspective of oxide metallurgy, fine MgO inclusions can strongly inhibit the growth of austenite grains, induce the nucleation of intracrystalline needle-shaped ferrite, and promote the formation of isocrystals and the refinement of the structure. Despite this, there are the following problems in controlling the inclusions in steel to high MgO content and pure MgO inclusions through magnesium treatment process: 1. Magnesium is an active metal with a low melting point. It will react violently during magnesium treatment, causing the magnesium element to volatilize, which will not only reduce the magnesium yield, but also may cause secondary oxidation of molten steel; 2. The process operation is difficult and the product quality is unstable; 3. If the amount of magnesium added during the magnesium treatment process is unreasonable or the process control is improper, there is also a risk of nozzle nodules, etc. This leads to certain limitations in using magnesium treatment process to control the inclusions in steel to high MgO content and pure MgO inclusions.

[0004] Based on the above reasons, the industry urgently needs to develop a refining slag system that can stably obtain high MgO content and pure MgO inclusions to solve the above problems and improve the cleanliness of molten steel and product quality. Summary of the invention

[0005] In order to overcome the above problems existing in the prior art, the present invention provides a refined slag system and application thereof, which are used to solve the above problems existing in the prior art.

[0006] A refined slag system is used for controlling the generation of high MgO content and pure MgO inclusions in the steelmaking process. The mass percentages of the components in the refined slag are CaO: 48.0-54.0%, Al2O3: 36.0-45.0%, MgO: 5.0-13.0%, SiO2 <3.0%, and the rest are inevitable impurities.

[0007] According to the above aspects and any possible implementation, there is further provided an implementation, wherein the mass ratio of CaO to Al2O3 in the refined slag is 1.1 to 1.4.

[0008] According to the aspects and any possible implementations described above, an implementation is further provided, wherein the mass percentages of the components in the refined slag are CaO: 48.0-52.1%, Al2O3: 36.0-42.9%, MgO: 5.0-13.0%, and SiO2<3.0%.

[0009] According to the aspects and any possible implementations described above, an implementation is further provided, wherein the mass percentages of the components in the refined slag are CaO: 48.6-52.1%, Al2O3: 36.3-42.9%, MgO: 6.0-12.2%, and SiO2<2.9%.

[0010] The present invention also provides an application of the refined slag system in a steelmaking process, comprising: a converter process: a high carbon drawing process is adopted at the end of a converter filled with a test steel grade, aluminum particles and a carburizer are added during the converter tapping process, and an alloy and the refined slag are added after the tapping is completed, wherein the amount of the refined slag added is 10-12 kg / ton of steel;

[0011] LF refining process: the electrode is heated to raise the temperature, and the refined slag added during the steel-making process is slag-made. During the entire LF refining process, the ladle is stirred by bottom blowing of argon gas, and the composition of the molten steel is fine-tuned, and the refining is carried out for a period of time;

[0012] RH vacuum treatment process: Under a certain RH vacuum degree, after a period of treatment, the T[O] content is lower than a certain amount after the vacuum is broken;

[0013] Billet continuous casting process: Billets are obtained through continuous casting.

[0014] According to the aspects and any possible implementations described above, there is further provided an implementation, wherein the test steel grade includes GCr15.

[0015] According to the above aspects and any possible implementation manner, there is further provided an implementation manner, wherein the alloy includes chromium, manganese and / or silicon.

[0016] According to the above aspects and any possible implementation, there is further provided an implementation, wherein the period of time is greater than 30 minutes.

[0017] According to the aspects and any possible implementation methods described above, an implementation method is further provided, wherein the RH vacuum degree is less than 30 Pa, the processing time is greater than or equal to 20 min, and the T[O] content after vacuum breaking is less than 6 ppm.

[0018] According to the above aspects and any possible implementation manner, an implementation manner is further provided, in which the size of the billet is 280 mm×320 mm.

[0019] Beneficial effects of the present invention

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] (1) It is possible to stably obtain high MgO content and pure MgO inclusions, and the inclusions are small in size and not easy to aggregate, but are dispersedly distributed, thereby improving the uniformity of the steel;

[0022] (2) The molten steel has a high degree of cleanliness, with T[O] in the molten steel less than 10ppm;

[0023] (3) Improved the castability of molten steel and the life of the ladle;

[0024] (4) The process is simple to operate and successfully solves problems such as violent reaction and secondary oxidation of molten steel, thereby improving the problem of unstable product quality. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 Schematic diagram of typical inclusion morphology and energy spectrum in the steel sample obtained in Experimental Example 1 of Example 1 of the present invention;

[0026] Figure 2 Schematic diagram of typical inclusion morphology and energy spectrum in the steel sample obtained in Experimental Example 2 of Example 1;

[0027] Figure 3 Schematic diagram of typical inclusion morphology and energy spectrum in the steel sample obtained in Experimental Example 3 of Example 1;

[0028] Figure 4 Schematic diagram of typical inclusion morphology and energy spectrum in the steel sample obtained in Experimental Example 4 in Example 1;

[0029] Figure 5 Schematic diagram of typical inclusion morphology and energy spectrum in the steel sample obtained in comparative test example 1 in embodiment 1;

[0030] Figure 6 Schematic diagram of typical inclusion morphology and energy spectrum in the steel sample obtained in Experimental Example 1 of Example 2;

[0031] Figure 7 Schematic diagram of typical inclusion morphology and energy spectrum in the steel sample obtained in Experimental Example 2 of Example 2;

[0032] Figure 8 Schematic diagram of the typical inclusion morphology and energy spectrum in the steel sample obtained in Experimental Example 3 in Example 2. DETAILED DESCRIPTION

[0033] In order to better understand the technical solution of the present invention, the content of the present invention includes but is not limited to the specific implementation methods described below, and similar technologies and methods should be considered to be within the scope of protection of the present invention. In order to make the technical problems, technical solutions and advantages to be solved by the present invention clearer, the following will be described in detail with reference to the accompanying drawings and specific embodiments.

[0034] It should be clear that the embodiments described in the present invention are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] The terms used in the embodiments of the present invention are only for the purpose of describing specific embodiments, and are not intended to limit the present invention. The singular forms "a", "said" and "the" used in the embodiments of the present invention and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.

[0036] The invention discloses a refined slag system for controlling the steelmaking process to generate high MgO content and pure MgO inclusions. The mass percentages of the components in the refined slag are CaO: 48.0-54.0%, Al2O3: 36.0-45.0%, MgO: 5.0-13.0%, SiO2<3.0%, and the rest are inevitable impurities.

[0037] CaO is one of the main components of refined slag, which can react with sulfur S in molten steel to form stable calcium sulfide CaS, which helps to remove S from molten steel. The higher the CaO in the slag, the greater the sulfur capacity of the slag and the stronger the desulfurization ability.

[0038] Al2O3 can lower the melting point of slag and improve its fluidity, which is very beneficial for desulfurization, deoxidation and removal of inclusions during the refining process. Especially at high temperatures, the appropriate Al2O3 content helps to adsorb non-metallic inclusions in molten steel, thereby purifying the molten steel and improving the cleanliness of the steel.

[0039] SiO2 can balance the content of basic oxides such as CaO and MgO in the slag, thereby adjusting the basicity of the slag. The appropriate SiO2 content helps to form a low-melting-point complex oxide with other oxide components in the slag, that is, to form a low-melting-point slag phase, which is beneficial to the floating and removal of inclusions in the molten steel.

[0040] MgO can protect the magnesia furnace lining, reduce the dissolution of the furnace lining into the slag (i.e. reduce the erosion of the furnace lining by the slag), and increase the service life of the furnace lining.

[0041] The refined slag has good desulfurization effect and inclusion removal ability while obtaining MgO inclusions, which is beneficial to improving the cleanliness of steel. In addition, it successfully solves the problems of violent reaction, secondary oxidation of molten steel and castability, and improves product quality.

[0042] Preferably, the mass ratio of CaO to Al2O3 in the refined slag is 1.1 to 1.4, and the slag can be completely slaged at the LF refining temperature (1550 to 1610°C), which can ensure that the refined slag has good solubility and fluidity, and the refined slag has a good adsorption capacity for inclusions in the molten steel, which can reduce the inclusion content in the molten steel. The specific mass ratio of CaO to Al2O3 can be 1.21, 1.27, 1.31 and 1.34.

[0043] Preferably, the mass percentage of each component in the refined slag is CaO: 48.0-52.1%, Al2O3: 36.0-42.9%, MgO: 5.0-13.0%, SiO2<3.0%. By appropriately reducing the content of CaO and Al2O3, the viscosity of the slag is reduced, the fluidity is significantly improved, the inclusion removal rate is significantly improved, and the cleanliness of the molten steel is further improved.

[0044] Preferably, the mass percentage of each component in the refined slag is CaO: 48.6-52.1%, Al2O3: 36.3-42.9%, MgO: 6.0-12.2%, SiO2<2.9%, while ensuring the cleanliness of the molten steel, the MgO and CaO in the slag are appropriately increased, and SiO2 is reduced, and the desulfurization capacity of the refined slag is enhanced. The MgO content in the slag reaches saturation, so that the MgO content in the inclusions is further increased, and the erosion of the refined slag on the refractory material is further weakened, thereby extending the service life of the ladle.

[0045] In the present invention, the mass ratio of CaO to Al2O3 is in the range of 1.1 to 1.4, and MgO is controlled to be 5.0 to 13.0% and SiO2 is less than 3.0%. The refined slag system after being jointly limited can control the generation of high MgO and pure MgO inclusions in the steel during the LF refining process. The MgO content in the inclusions exceeds 92%. At the same time, the molten steel can obtain a very high cleanliness, and the oxygen content in the steel can be controlled to be below 0.0010%.

[0046] As an embodiment disclosed by the present invention, the present invention further provides an application of the refined slag system of the present invention in a steelmaking process, comprising: a converter process: a high carbon drawing process is adopted at the end of a converter filled with a test steel grade, aluminum particles and a carburizer are added during the converter tapping process, and an alloy and the refined slag are added after the tapping is completed, wherein the amount of the refined slag added is 10-12 kg / ton of steel;

[0047] LF refining process: the electrode is heated to raise the temperature, and the refined slag added during the steel-making process is slag-made. During the entire LF refining process, the ladle is stirred by bottom blowing of argon gas, and the composition of the molten steel is fine-tuned, and the refining is carried out for a period of time;

[0048] RH vacuum treatment process: Under a certain RH vacuum degree, after a period of treatment, the T[O] content is lower than a certain amount after the vacuum is broken;

[0049] Billet continuous casting process: Billets are obtained through continuous casting.

[0050] The test steel type includes GCr15 or Q420qd; the alloy includes chromium, manganese and / or silicon; the period of time is greater than 30 minutes; the RH vacuum degree is less than 30Pa, the processing time is greater than or equal to 20 minutes, the T[O] content after vacuum breaking is less than 6ppm, and the size of the final square billet is 280mm×320mm. The following examples are used to illustrate the specifics:

[0051] Embodiment 1

[0052] In the following examples, the test steel type is GCr15, and its chemical composition is shown in Table 1. The number of furnaces implemented is 5, and the chemical composition of the refined slag in the 5 furnaces is shown in Table 2. The test process can adopt the common bearing steel production process in this field, that is, 120t converter → LF refining → RH vacuum treatment → billet continuous casting.

[0053] Converter process: The converter end point adopts high carbon drawing process, and aluminum particles and carburizer are added during the converter tapping process. After the tapping is completed, most alloys (such as chromium, manganese, silicon, etc.) and the refined slag designed by the present invention are added. The addition of alloys makes the content of each element in the molten steel reach or approach the standard of finished bearing steel. The amount of refined slag added is 10-12 kg / ton of steel.

[0054] LF refining process: the electrode is heated to raise the temperature, and the refined slag added during the steel-making process is slag-made. During the entire LF refining process, the ladle is stirred with argon gas at the bottom, and the composition of the molten steel is fine-tuned to meet the requirements of the finished product. Refining time> 30min.

[0055] RH vacuum treatment process: RH vacuum degree is required to be less than 30Pa, the treatment time is not less than 20min, and the T[O] content after vacuum breaking is required to be less than 6ppm.

[0056] Billet continuous casting process: 280mm×320mm billets are obtained through continuous casting.

[0057] Test Example 1: In this test example, the refined slag added to the ladle is the 1# refined slag in Table 2.

[0058] Test Example 2: In this test example, the refined slag added to the ladle is the 2# refined slag in Table 2.

[0059] Test Example 3: In this test example, the refined slag added to the ladle is the 3# refined slag in Table 2.

[0060] Test Example 4: In this test example, the refined slag added to the ladle is the 4# refined slag in Table 2.

[0061] Comparative Test Example 1: In this test example, the refined slag added to the ladle is 5# refined slag in Table 2 (conventional refined slag).

[0062] The square billets obtained in the above examples were respectively taken to analyze the non-metallic inclusions in the steel. Figure 1 , Figure 2 , Figure 3 and Figure 4 , respectively, are the typical inclusion morphology and energy spectrum of the steel samples obtained in Test Examples 1, 2, 3 and 4. It can be seen that the inclusions in the steel samples obtained in industrial production using the refined slag designed by the present invention are MgO, and the inclusion size is less than 5μm. As shown in Table 3, detailed information on inclusions and molten steel cleanliness in Test Examples 1, 2, 3 and 4 is shown. It can be seen that the inclusions in the steel samples obtained using the refined slag designed by the present invention are all pure MgO and high MgO content inclusions, and the inclusion size is very small, with an average size of about 2μm. At the same time, the molten steel has a very high cleanliness, and T[O] in the molten steel is less than ≤5ppm. In addition, long-term production time shows that the castability of the molten steel is significantly improved by using the refined slag designed by the present invention, and continuous casting of more than 8 furnaces can be easily achieved, and the service life of the ladle is doubled.

[0063] See also Figure 5 , which is the typical inclusion morphology and energy spectrum in the steel sample obtained in Comparative Test Example 1, it can be seen that the inclusions in the steel sample are CaO-MgO-Al2O3. See Table 4 for detailed information on inclusions and steel liquid cleanliness in Comparative Test Example 1. It can be seen that the inclusions in the steel sample obtained in Comparative Test Example 1 are mainly MgO-Al2O3 and CaO-Al2O3-MgO inclusions, and the average size and T[O] content are greater than the steel sample obtained using the refined slag designed by the present invention.

[0064] Table 1 Composition of steel grade GCr15 in Example 1, mass percentage

[0065] C Si Mn Cr S GCr15 1.0 0.2 0.4 1.5 0.020

[0066] Table 2 Composition of refined slag used in Example 1, mass percentage

[0067] Group No. CaO <![CDATA[Al2O3]]> MgO <![CDATA[SiO2]]> 1# 52.1 42.9 5.0 0 2# 51.3 40.4 7.1 1.2 3# 50.2 38.4 9.3 2.1 4# 48.6 36.3 12.2 2.9 5# 55.8 32.1 4.9 7.2

[0068] Table 3 Detailed information on inclusions and steel cleanliness in the test examples

[0069]

[0070] Table 4 Detailed information on inclusions and cleanliness of molten steel in comparative test example 1

[0071]

[0072] Embodiment 2

[0073] In the following examples, the experimental steel type is Q420qd, and its chemical composition is shown in Table 5. The number of furnaces implemented is 3, and the chemical composition of the refined slag in the 3 furnaces is shown in Table 6. The experimental process can adopt the conventional laboratory steel-slag reaction, that is, base iron material preparation, slag material design and preparation, and steel-slag reaction. The experimental process used in the following examples is specifically described as follows:

[0074] Preparation of base iron material: The base iron material is obtained by smelting in a vacuum induction furnace. When smelting the base iron material, firstly, industrial pure iron is smelted in a vacuum electromagnetic induction furnace, and then, alloy raw materials are added to the molten steel through a feeding bin under vacuum conditions to adjust the content of each element in the molten steel.

[0075] Slag design and preparation: The refined slag used in the experiment is made of CaO, Al2O3, MgO, SiO2 chemically pure raw materials. Then the refined slag composition designed in accordance with the present invention is prepared and fully stirred and mixed.

[0076] Steel-slag reaction: The refined slag and steel designed by the present invention are charged into a MgO crucible, and then slag-steel refining is performed.

[0077] Test Example 1: In this test example, the refined slag added to the ladle is the 1# refined slag in Table 6.

[0078] Test Example 2: In this test example, the refined slag added to the ladle is the 2# refined slag in Table 6.

[0079] Test Example 3: In this test example, the refined slag added to the ladle is the 3# refined slag in Table 6.

[0080] Take the steel samples obtained from the above steel-slag reaction and analyze the non-metallic inclusions in the steel. Figure 6 , Figure 7 and Figure 8 , which are the typical inclusion morphology and energy spectrum in the steel sample obtained in Example 2. It can be seen that the inclusions in the steel sample obtained under laboratory conditions using the refined slag designed by the present invention are MgO, and the inclusion size is less than 5μm. See Table 7 for detailed information on the inclusions and cleanliness of the molten steel in the steel sample obtained in Example 2. It can be seen that the inclusions in the steel sample obtained using the refined slag designed by the present invention are all pure MgO and high MgO content inclusions, and the inclusion size is very small, with an average size of about 2μm. At the same time, the molten steel has a very high cleanliness, and T[O] in the molten steel is less than 10ppm.

[0081] Table 5 Composition of steel grade Q420qd in Example 2, mass percentage

[0082] C Si Mn P S Q420 0.11 0.50 1.70 0.029 0.022

[0083] Table 6 Composition of refined slag used in Example 2, mass percentage

[0084] Group No. CaO <![CDATA[Al2O3]]> MgO <![CDATA[SiO2]]> 1# 52.0 42.0 6.0 0 2# 50.0 41.0 8.0 1.0 3# 49.0 39.0 10.0 2.0

[0085] Table 7 Detailed information on inclusions and steel liquid cleanliness in Example 2

[0086]

[0087] In summary, the refined slag designed by the present invention can stably obtain pure MgO and high MgO content inclusions both under laboratory conditions and in industrial production. Such inclusions are very small in size, not easy to aggregate, and are dispersedly distributed, which is beneficial to improving the uniformity of steel. At the same time, the molten steel has a high degree of cleanliness, T[O] in the molten steel is less than 10ppm, and the castability of the molten steel and the life of the ladle are effectively improved in industrial production. In addition, the method is simple in process operation, and successfully solves the problems of violent reaction, secondary oxidation of molten steel, etc., thereby improving the problem of unstable product quality.

[0088] The above description shows and describes several preferred embodiments of the present invention, but as mentioned above, it should be understood that the present invention is not limited to the form disclosed herein, and should not be regarded as excluding other embodiments, but can be used in various other combinations, modifications and environments, and can be modified within the scope of the application concept described herein through the above teachings or the technology or knowledge of the relevant field. The changes and modifications made by those skilled in the art shall not depart from the spirit and scope of the present invention, and shall be within the scope of protection of the claims attached to the present invention.

Claims

1. A refined slag system for controlling the generation of high MgO content and pure MgO inclusions in the steelmaking process. Features: The mass percentages of the components in the refined slag are CaO: 48.0-54.0%, Al 2 O 3 :36.0~45.0%, MgO: 5.0~13.0%, SiO 2 <3.0%, the rest are inevitable impurities.

2. The refined slag system according to claim 1, It is characterized in that The CaO and Al in the refined slag 2 O 3 The mass ratio is 1.1 to 1.

4.

3. The refined slag system according to claim 1, It is characterized in that The mass percentages of the components in the refined slag are CaO: 48.0-52.1%, Al 2 O 3 :36.0~42.9%, MgO: 5.0~13.0%, SiO 2 <3.0%.

4. The refined slag system according to claim 2, It is characterized in that The mass percentage of each component in the refined slag is CaO: 48.6-52.1%, Al 2 O 3 :36.3~42.9%, MgO: 6.0~12.2%, SiO 2 <2.9%.

5. Use of the refined slag system according to any one of claims 1 to 4 in a steelmaking process, It is characterized in that The process comprises: a converter process: a high carbon drawing process is adopted at the end of the converter filled with the test steel, aluminum particles and a carburizer are added during the steel tapping process of the converter, and alloy and the refined slag are added after the steel tapping is completed, and the amount of the refined slag added is 10-12 kg / ton of steel; LF refining process: the electrode is heated to raise the temperature, and the refined slag added during the steel-making process is slag-made. During the entire LF refining process, the ladle is stirred by bottom blowing of argon gas, and the composition of the molten steel is fine-tuned, and the refining is carried out for a period of time; RH vacuum treatment process: Under a certain RH vacuum degree, after a period of treatment, the T[O] content is lower than a certain amount after the vacuum is broken; Billet continuous casting process: Billets are obtained through continuous casting.

6. The use according to claim 5, It is characterized in that The test steel grades include GCr15.

7. The use according to claim 5, It is characterized in that The alloy includes chromium, manganese and / or silicon.

8. The use according to claim 5, It is characterized in that The period of time is greater than 30 minutes.

9. The use according to claim 5, It is characterized in that The RH vacuum degree is less than 30 Pa, the processing time is greater than or equal to 20 minutes, and the T[O] content after vacuum breaking is less than 6 ppm.

10. The use according to claim 5, It is characterized in that The size of the billet is 280 mm×320 mm.

Citation Information

Patent Citations

  • Refining slag for bearing steel production and smelting process of refining slag

    CN106435093A

  • Smelting method of low-cost high-purity 60Si2Mn spring steel

    CN111485062A

  • Refining slag system suitable for producing bearing steel by 120-ton refining furnace

    CN114635016A

  • Smelting method for removing inclusions in steel

    CN115287406A

  • Control method for B-type inclusions in high-carbon chromium bearing steel