Porous transmission layer and preparation method and application thereof

Through vacuum coating technology, the combination of non-precious metal and precious metal coatings on the porous transport layer is solved, and the problems of high cost, unenvironmental and low porosity of the preparation method in the prior art are achieved, and efficient and environmentally friendly porous transport layer preparation is achieved to meet the needs of the Performance requirements for PEM electrolyzed water.

CN119020735AInactive Publication Date: 2024-11-26CEMT CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411496232.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-25
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing porous transport layer preparation methods have problems such as high cost, unecotch environmental protection, low production efficiency, low porosity and uneven coating, which limits its performance in practical applications.

Method used

The porous transport layer is prepared by vacuum coating technology. By combining non-precious metal conductive layer and precious metal coating on the substrate, the ion plating process is used to ensure the uniformity and bonding force of the coating, reduce the thickness of the precious metal coating to reduce costs, and avoid electroplating. and environmental pollution caused by brushing.

Benefits of technology

The conductivity of the porous transport layer and the performance consistency of the wet plating Pt process is achieved. The contact resistance is close to that of commercial electroplating Pt, and the porosity reaches more than 68%, which meets the performance requirements of PEM electrolytic water, reducing production costs and environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020735A_ABST
    Figure CN119020735A_ABST
Patent Text Reader

Abstract

The invention provides a porous transmission layer and a preparation method and application thereof. The preparation method comprises the following steps: (1) carrying out glow cleaning on a base material; and (2) carrying out vacuum coating treatment on the substrate subjected to glow cleaning, and cooling to obtain the porous transmission layer, wherein the vacuum coating treatment comprises the following steps: coating a base material with a non-noble metal coating, and then coating the non-noble metal coating with a noble metal. The PEM electrolytic cell porous transmission layer is prepared by adopting a vacuum coating technology, the porous transmission layer prepared by the method is more uniform in coating thickness and better in product performance consistency, the vacuum coating technology belongs to the series of dry coating, the waste liquid problem caused by electroplating or brush coating in the industry is avoided, the use of toxic organic solvents is reduced, and the production cost is reduced. And pollution to the environment is avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of proton exchange membrane water electrolysis and relates to a porous transmission layer and a preparation method and application thereof. Background Art

[0002] The porous transport layer of the PEM electrolyzer is mainly composed of titanium felt, titanium mesh or other porous metal mesh, which provides the functions of conducting electrons, water flow channels and catalyst carriers. The porous transport layer of the PEM electrolyzer has high requirements for corrosion resistance, conductivity, stability and porosity.

[0003] Titanium is the most popular material for the porous transport layer. However, the physical and chemical properties of titanium make it very easy to oxidize in the working environment of the PEM electrolyzer, resulting in reduced conductivity of the porous transport layer, which in turn has a great negative impact on the performance of the electrolyzer.

[0004] In order to solve the above problems, it is necessary to add a coating protection to the porous transmission layer. It is required that the addition of the coating should not affect the porosity of the porous transmission layer, the cost of the coating should be within a reasonable range, the production process of the coating should be environmentally friendly and less polluting, and the processing and manufacturing process of the coating should be short and efficient.

[0005] Traditional porous transport layers are generally electroplated, brushed or sprayed with precious metals. Due to the placement of the porous transport layer and the porous structure, the electroplated coating will have uneven charge distribution during the electroplating process, resulting in uneven coating and environmental damage. The spraying or brushing sintering process has a high temperature, which causes great damage to the porous transport layer, resulting in low porosity and affecting the installation and actual performance of the porous transport layer.

[0006] CN116949477A discloses a method for preparing a porous transport layer, a porous transport layer and a proton exchange membrane water electrolyzer, wherein the method comprises: firstly, degreasing and deoiling a metal foil having high conductivity and high corrosion resistance as a base material, and after ultrasonic cleaning and drying, performing elongated straight-through hole forming processing on the basis of the metal foil according to set parameters to obtain a porous transport layer.

[0007] CN116334674A discloses a PEM water electrolysis cathode porous transport layer and a preparation method thereof, wherein the method comprises the following steps: step one: using high-pressure steam to enter the carbon support layer, opening the microporous structure of the carbon support layer, and obtaining a pore-enlarged carbon support layer; step two: preparing a non-precious metal compound solution, and heating the non-precious metal compound solution to form non-precious metal compound vapor; step three: intermittently contacting the non-precious metal compound vapor with the pore-enlarged carbon support layer, so that the non-precious metal compound vapor is intermittently deposited on the pore-enlarged carbon support layer, and during the time when the non-precious metal compound vapor stops contacting the pore-enlarged carbon support layer, the pore-enlarged carbon support layer is laser irradiated to finally obtain a cathode porous transport layer.

[0008] The method for preparing the porous transport layer in the above scheme has the problems of high cost, environmental pollution and low production efficiency. In addition, the porosity of the prepared porous transport layer is low and the coating is uneven, which limits its application in practice. Summary of the invention

[0009] The purpose of the present invention is to provide a porous transmission layer and a preparation method and application thereof. The present invention adopts vacuum coating technology to prepare a porous transmission layer of a PEM electrolytic cell. The porous transmission layer prepared by the method has a more uniform coating thickness and better product performance consistency. The vacuum coating process belongs to the category of dry coating, which avoids the waste liquid problem caused by electroplating or brushing in the industry, reduces the use of toxic organic solvents, and avoids pollution to the environment.

[0010] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0011] In a first aspect, the present invention provides a method for preparing a porous transport layer, the preparation method comprising the following steps:

[0012] (1) Glow cleaning of the substrate;

[0013] (2) vacuum coating the glow-cleaned substrate, and obtaining the porous transmission layer after cooling;

[0014] The vacuum coating process includes coating a non-precious metal coating on a substrate and then coating a precious metal on the non-precious metal coating.

[0015] After the porous transmission layer substrate is activated by inert gas plasma cleaning, the present invention uses a vacuum coating process to coat the non-precious metal conductive layer. The non-precious metal layer has a ceramic coating or a pure metal coating with high conductivity. Due to the use of the ion plating process, the ions have good diffraction properties and can be well deposited into the internal space of the porous transmission layer, and due to the bombardment of high-energy ions, the bonding force of the coating is relatively large. The precious metal coating mainly coats a layer of precious metal on the surface of the non-precious metal coating. The thickness of the precious metal film layer is relatively low and can be evenly distributed on the surface of the porous transmission layer, playing a conductive and corrosion-resistant role. The entire coating process is simple to operate, and the coating time is within 1 hour. Dozens of gas transmission layers can be plated at a time, and the production efficiency is high.

[0016] Preferably, the substrate in step (1) comprises any one of titanium mesh, titanium felt, titanium porous plate, metal mesh or composite porous conductive material, or a combination of at least two thereof.

[0017] Preferably, pretreatment is performed before the glow cleaning in step (1).

[0018] Preferably, the pretreatment includes degreasing-water washing-acid washing-water washing-vacuum drying.

[0019] Preferably, the mass concentration of the degreasing agent used for degreasing is 0.1-1%, for example, 0.1%, 0.2%, 0.5%, 0.8% or 1%.

[0020] Preferably, the degreasing time is 2 to 10 min, for example, 2 min, 4 min, 6 min, 8 min or 10 min.

[0021] Preferably, the pickling solution for pickling comprises any one of oxalic acid, nitric acid or hydrofluoric acid or a combination of at least two thereof, preferably a mixed acid solution of oxalic acid, nitric acid and hydrofluoric acid.

[0022] Preferably, the pickling time is 5 to 20 minutes, for example, 5 minutes, 8 minutes, 10 minutes, 15 minutes or 20 minutes.

[0023] Preferably, the temperature of the vacuum drying is 60-150°C, for example, 60°C, 80°C, 100°C, 120°C or 150°C.

[0024] Preferably, the vacuum degree of the vacuum drying is 1-100 Pa, for example, 1 Pa, 5 Pa, 10 Pa, 40 Pa or 100 Pa.

[0025] Preferably, the vacuum drying time is 20 to 40 min, for example, 20 min, 25 min, 30 min, 35 min or 40 min.

[0026] Preferably, the washing time is independently 1 to 3 min, for example, 1 min, 1.5 min, 2 min, 2.5 min or 3 min.

[0027] Preferably, the glow cleaning in step (1) comprises cleaning the substrate in an inert atmosphere by means of negative glow discharge and an ion source.

[0028] Preferably, the bias voltage of the glow cleaning is 500-1000V, for example, 500V, 600V, 700V, 800V or 1000V.

[0029] Preferably, the pressure of the inert atmosphere is 0.1-100 Pa, for example, 0.11 Pa, 5 Pa, 10 Pa, 40 Pa or 100 Pa, etc., preferably 0.1-10 Pa.

[0030] Preferably, the ion source comprises any one of an anode layer ion source, a Hall ion source, a Kaufman ion source or a plasma source, or a combination of at least two thereof.

[0031] Preferably, the ion beam energy of the ion source is 100-500 eV, for example, 100 eV, 200 eV, 300 eV, 400 eV or 500 eV.

[0032] Preferably, the cleaning time of the ion source is 5 to 30 min, for example, 5 min, 10 min, 15 min, 20 min or 30 min.

[0033] Preferably, the vacuum coating treatment device in step (2) comprises a single vacuum coating furnace and / or a continuous vacuum coating furnace.

[0034] Preferably, the vacuum coating treatment method includes any one of vacuum evaporation, multi-arc ion plating, PECVD or magnetron sputtering, or a combination of at least two thereof, preferably multi-arc ion plating.

[0035] The present invention adopts a reasonable ion plating process, the diffraction of ions is better, the uneven brushing is solved, and the occurrence of no coating inside the porous transmission layer is avoided.

[0036] Preferably, the cooling time in step (2) is 3 to 20 min, for example, 3 min, 5 min, 10 min, 15 min or 20 min, etc., preferably 5 to 10 min.

[0037] Preferably, the cooling atmosphere comprises nitrogen and / or argon.

[0038] Preferably, the non-precious metal target material includes any one of Ti, Cr, W or Nb, or a combination of at least two of them.

[0039] Preferably, the non-precious metal coating is deposited by a coating method including multi-arc ion plating and / or PECVD.

[0040] Preferably, the coating bias voltage of the non-precious metal coating is 50-500V, for example, 50V, 100V, 200V, 300V or 500V, etc., preferably 100-300V.

[0041] Preferably, the gas pressure of the non-precious metal coating film is 0.1~10Pa, for example: 0.1 Pa, 1 Pa, 2 Pa, 5Pa or 10 Pa, etc., preferably 1~3Pa.

[0042] Preferably, the coating gas for coating the non-precious metal coating includes any one of argon, nitrogen or methane, or a combination of at least two of them.

[0043] Preferably, the coating temperature of the non-precious metal coating is 60-600°C, for example, 60°C, 100°C, 200°C, 400°C or 600°C, etc., preferably 100-400°C.

[0044] Preferably, the coating time of the non-precious metal coating is 5 to 20 minutes, for example, 5 minutes, 8 minutes, 10 minutes, 15 minutes or 20 minutes.

[0045] Preferably, the noble metal target material includes any one of Au, Pt, Ta or Ir, or a combination of at least two of them.

[0046] Preferably, the noble metal coating method includes multi-arc ion plating.

[0047] Preferably, the noble metal coating bias voltage is 50-500V, for example, 50V, 100V, 200V, 300V or 500V, etc., preferably 100-300V.

[0048] Preferably, the gas pressure of the precious metal coating is 0.1~10Pa, for example: 0.1 Pa, 1 Pa, 2 Pa, 5 Pa or 10Pa, etc., preferably 1~3Pa.

[0049] Preferably, the temperature of the precious metal coating is 60-600°C, for example, 60°C, 100°C, 200°C, 400°C or 600°C, etc., preferably 100-300°C.

[0050] Preferably, the precious metal coating time is 1 to 5 minutes, for example, 1 minute, 2 minutes, 3 minutes, 4 minutes or 5 minutes.

[0051] In a second aspect, the present invention provides a porous transport layer, which is prepared by the method described in the first aspect, and comprises a substrate and a non-precious metal film layer and a precious metal film layer sequentially stacked on at least one side of the substrate.

[0052] The porous transmission layer prepared by the present invention has a non-precious metal film layer + precious metal film layer structure. Under the premise of ensuring good overall conductivity and corrosion resistance, the thickness of the precious metal coating can be greatly reduced. The thickness of the precious metal only needs to be 1 / 2 of that of other processes, which greatly reduces the cost of the porous transmission layer.

[0053] Preferably, the thickness of the non-precious metal film layer is 100-500 nm, for example, 100 nm, 200 nm, 300 nm, 400 nm or 500 nm.

[0054] Preferably, the material of the non-precious metal film layer includes any one of Ti, Cr, Nb, W, and their nitrides, carbides or carbonitrides, or a combination of at least two thereof.

[0055] Preferably, the thickness of the noble metal film layer is 20-100 nm, for example, 20 nm, 40 nm, 60 nm, 80 nm or 100 nm.

[0056] Preferably, the material of the noble metal film layer includes any one of Au, Pt, Ta or Ir, or a combination of at least two of them.

[0057] In a third aspect, the present invention provides a PEM electrolyzer, wherein the PEM electrolyzer comprises the porous transport layer as described in the second aspect.

[0058] Compared with the prior art, the present invention has the following beneficial effects:

[0059] (2) The conductive properties of the porous transport layer prepared by the present invention are consistent with those of the wet Pt plating process, and the contact resistance is close to or even better than that of the gas transport layer of commercial Pt electroplating. In terms of water electrolysis performance, it is consistent with the traditional commercial porous transport layer and fully meets the performance requirements of the porous transport layer of existing PEM water electrolysis.

[0060] (3) The porosity of the porous transport layer prepared by the method of the present invention can reach more than 68%, and the contact resistance can reach 3.8 mΩ·cm 2 Below, the corrosion current density can reach 1.3μA / cm 2 Below, performance tests in a PEM electrolyzer show that at 1.6A / cm 2 The voltage can reach below 1.85V at a current density of . BRIEF DESCRIPTION OF THE DRAWINGS

[0061] Figure 1 This is an optical microscope image of the PVD-coated titanium felt described in Example 1.

[0062] Figure 2 This is an optical microscope image of the electroplated titanium felt described in Comparative Example 1.

[0063] Figure 3 It is a schematic diagram of the structure of the porous transmission layer prepared in Example 1 of the present invention, 201-substrate, 202-non-precious metal film layer, 203-precious metal film layer.

[0064] Figure 4 It is a schematic diagram of the pretreatment device described in the embodiment of the present invention, 101-degreasing tank, 102 pure water tank, 103-pickling tank, 104-pure water tank, 105-vacuum drying oven.

[0065] Figure 5 It is a schematic diagram of the coating device described in the embodiment of the present invention, 301-pre-vacuum chamber, 302-ion cleaning chamber, 303-non-precious metal coating chamber, 304-precious metal coating chamber, 305-cooling chamber.

[0066] Figure 6 A comparison diagram of the contact resistance of the porous transport layers prepared in Examples 1-3 of the present invention and Comparative Example 1.

[0067] Figure 7 It is a comparison chart of the performance test of the PEM electrolyzer with porous transport layers prepared in Example 1 of the present invention and Comparative Example 1. DETAILED DESCRIPTION

[0068] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0069] Example 1

[0070] This embodiment provides a porous transmission layer, and the preparation method of the porous transmission layer is as follows:

[0071] (1) A titanium felt with an area of ​​10 cm×10 cm and a thickness of 0.25 mm is selected as a substrate, and the titanium felt is pretreated. The schematic diagram of the pretreatment device is shown in FIG. Figure 4As shown, the titanium felt is placed in a degreasing tank 101 containing 0.1% degreasing agent at a temperature of 60°C and ultrasonically cleaned for 5 minutes. After degreasing, the titanium felt is immediately moved to a pure water tank 102 for cleaning for 2 minutes; then the titanium felt is moved to a pickling tank 103 containing 1% oxalic acid, 0.05% HF and 0.5% HNO3 for corrosion for 10 minutes; after pickling, it is immediately transferred to a pure water tank 104 for cleaning for 2 minutes; finally, the titanium felt is moved to a vacuum drying oven 105 for drying at 80°C for 30 minutes;

[0072] (2) The pre-treated substrate is placed on the material rack of the PVD furnace and placed in the furnace for coating. The schematic diagram of the coating treatment device is as follows: Figure 5 As shown, the pre-vacuum chamber 301 is roughly evacuated, and then moved to the ion cleaning chamber 302. When the background vacuum degree reaches 1×10 -2 After 100 Pa, 300 sccm of Ar gas was introduced, and glow cleaning was performed at a pressure of 10 Pa and a bias voltage of 800 V. The ion source was cleaned at the same time of glow cleaning. The ion source cleaning power was 2.4 KW, the energy of the ion beam was 200 eV, and the cleaning time was 15 min.

[0073] (3) The titanium felt after glow cleaning is transferred to the non-precious metal coating chamber 303 for multi-arc ion plating, and a Ti target is used for coating. During the coating process, 300 sccm of nitrogen is introduced, the coating temperature is 270°C, the gas pressure is 5Pa, the bias voltage is selected to be 300V, and the coating time is 20min. A TiN coating is formed on the titanium felt, and the titanium felt sample is transferred to the precious metal coating chamber 304. A precious metal Pt target is used for coating. 100 sccm of argon is used for coating. The gas pressure is 3Pa, the bias voltage is 250V, the coating temperature is 180°C, and the coating time is 5min. The titanium felt plated with precious metals is transferred to the cooling chamber 305 for cooling. During the cooling process, 50 sccm of nitrogen is introduced, and the cooling time is 5min. After cooling, the furnace inspection is carried out to obtain the porous transmission layer. The optical microscope image of the porous transmission layer is as shown in the figure Figure 1 As shown, the schematic structural diagram of the porous transmission layer is as follows Figure 3 As shown, the thickness of the substrate 201 is 250 nm, the thickness of the non-precious metal film layer 202 is 300 nm, and the thickness of the precious metal film layer 203 is 80 nm.

[0074] Example 2

[0075] This embodiment provides a porous transmission layer, and the preparation method of the porous transmission layer is as follows:

[0076] (1) A titanium felt with an area of ​​10 cm×10 cm and a thickness of 0.25 mm is selected as a substrate, and the titanium felt is pretreated. The schematic diagram of the pretreatment device is shown in FIG. Figure 4As shown, the titanium felt is placed in a degreasing tank 101 containing 2% degreasing agent at a temperature of 60°C and ultrasonically cleaned for 5 minutes. After degreasing, the titanium felt is immediately moved to a pure water tank 102 for cleaning for 1.5 minutes; then the titanium felt is moved to a pickling tank 103 containing 1% oxalic acid, 0.05% HF and 0.5% HNO3 for corrosion for 5 minutes; after pickling, it is immediately transferred to a pure water tank 104 for cleaning for 2.5 minutes; finally, the titanium felt is moved to a vacuum drying oven 105 for drying at 60°C for 40 minutes;

[0077] (2) The pre-treated substrate is placed on the material rack of the PVD furnace and placed in the furnace for coating. The schematic diagram of the coating treatment device is as follows: Figure 5 As shown, the pre-vacuum chamber 301 is roughly evacuated, and then moved to the ion cleaning chamber 302. When the background vacuum degree reaches 1×10 -2 After 100 Pa, 300 sccm of Ar gas was introduced, and glow cleaning was performed at a pressure of 100 Pa and a bias of 500 V. The ion source was cleaned at the same time of glow cleaning. The ion source cleaning power was 2KW, the energy of the ion beam was 100eV, and the cleaning time was 30 minutes;

[0078] (3) The titanium felt after glow cleaning is transferred to the non-precious metal coating chamber 303 for PECVD coating, and the Ti target is used for coating. During the coating process, 300sccm of nitrogen is introduced, the coating temperature is 250°C, the gas pressure is 1Pa, the bias voltage is selected to be 100V, and the coating time is 15min. A TiN coating is formed on the titanium felt. The titanium felt sample is transferred to the precious metal coating chamber 304 and coated with the precious metal Pt target. The coating is carried out with 100sccm of argon gas, the coating temperature is 200°C, the gas pressure is 1Pa, the bias voltage is 150V, and the coating time is 3min. The titanium felt coated with the precious metal is transferred to the cooling chamber 305 for cooling. During the cooling process, 50sccm of nitrogen is introduced, and the cooling time is 5min. After cooling, the furnace inspection is carried out to obtain the porous transmission layer. The thickness of the non-precious metal film layer in the porous transmission layer is 240nm, and the thickness of the precious metal film layer is 50nm.

[0079] Example 3

[0080] This embodiment provides a porous transmission layer, and the preparation method of the porous transmission layer is as follows:

[0081] (1) A titanium felt with an area of ​​10 cm×10 cm and a thickness of 0.25 mm is selected as a substrate, and the titanium felt is pretreated. The schematic diagram of the pretreatment device is shown in FIG. Figure 4As shown, the titanium felt is placed in a degreasing tank 101 containing 1% degreasing agent at a temperature of 60°C and ultrasonically cleaned for 2 minutes. After degreasing, the titanium felt is immediately moved to a pure water tank 102 for cleaning for 3 minutes; then the titanium felt is moved to a pickling tank 103 containing 1% oxalic acid, 0.05% HF and 0.5% HNO3 for corrosion for 20 minutes; after pickling, it is immediately transferred to a pure water tank 104 for cleaning for 3 minutes; finally, the titanium felt is moved to a vacuum atmosphere protection furnace and dried at 150°C for 20 minutes;

[0082] (2) The pre-treated substrate is placed on the material rack of the PVD furnace and placed in the furnace for coating. The schematic diagram of the coating treatment device is as follows: Figure 5 As shown, the pre-vacuum chamber 301 is roughly evacuated, and then moved to the ion cleaning chamber 302. When the background vacuum degree reaches 1×10 -2 After 1.5 Pa, 300 sccm of Ar gas was introduced, and glow cleaning was performed at a pressure of 0.1 Pa and a bias voltage of 1000 V. The ion source was cleaned at the same time of glow cleaning. The ion source cleaning power was 2KW, the energy of the ion beam was 500eV, and the cleaning time was 5min;

[0083] (3) The titanium felt after glow cleaning is transferred to the non-precious metal coating chamber 303 for vacuum evaporation, and the Ti target is used for coating. During the coating process, 300 sccm of nitrogen is introduced, the coating temperature is 250°C, the gas pressure is 3Pa, the bias voltage is selected to be 100V, and the coating time is 5min. A TiN coating is formed on the titanium felt. The titanium felt sample is transferred to the precious metal coating chamber 304 and coated with the precious metal Pt target. The coating is carried out with 100 sccm of argon gas, the coating temperature is 200°C, the gas pressure is 3Pa, the bias voltage is 100V, and the coating time is 1min. The titanium felt coated with the precious metal is transferred to the cooling chamber 305 for cooling. During the cooling process, 50 sccm of nitrogen is introduced, and the cooling time is 5min. After cooling, the furnace inspection is carried out to obtain the porous transmission layer. The thickness of the non-precious metal film layer in the porous transmission layer is 100nm, and the thickness of the precious metal film layer is 20nm.

[0084] Example 4

[0085] The difference between this embodiment and embodiment 1 is that the bias voltage of the non-precious metal coating and the precious metal coating is 50V, and the other conditions and parameters are exactly the same as those in embodiment 1.

[0086] Example 5

[0087] The difference between this embodiment and embodiment 1 is that the bias voltage of the non-precious metal coating and the precious metal coating is 500V, and the other conditions and parameters are exactly the same as those in embodiment 1.

[0088] Example 6

[0089] The only difference between this embodiment and embodiment 1 is that the temperature of the non-precious metal coating and the precious metal coating is 60° C., and the other conditions and parameters are exactly the same as those in embodiment 1.

[0090] Example 7

[0091] The only difference between this embodiment and the first embodiment is that the temperature of the non-precious metal coating and the precious metal coating is 600° C., and the other conditions and parameters are exactly the same as those of the first embodiment.

[0092] Example 8

[0093] The only difference between this embodiment and embodiment 1 is that the pressure of the non-precious metal coating and the precious metal coating is 0.1 Pa, and the other conditions and parameters are exactly the same as those in embodiment 1.

[0094] Example 9

[0095] The only difference between this embodiment and embodiment 1 is that the pressure of the non-precious metal coating and the precious metal coating is 10 Pa, and the other conditions and parameters are exactly the same as those in embodiment 1.

[0096] Comparative Example 1

[0097] The only difference between this comparative example and Example 1 is that conventional electroplating is used instead of multi-arc ion plating, and other conditions and parameters are exactly the same as those in Example 1. Figure 2 shown.

[0098] Comparative Example 2

[0099] The only difference between this comparative example and Example 1 is that no non-precious metal layer is provided, and other conditions and parameters are exactly the same as those in Example 1.

[0100] Comparative Example 3

[0101] The only difference between this comparative example and Example 1 is that no noble metal layer is provided, and other conditions and parameters are exactly the same as those in Example 1.

[0102] Performance Test:

[0103] The porous transport layer prepared in the embodiment and the comparative example was tested for porosity, contact resistance and corrosion current density. The contact resistance was tested using a low resistance tester, the test pressure was 1.5 MPa, and the test points were at least 3 positions. The porosity was tested using mercury intrusion. The corrosion current density test was tested using an electrochemical workstation, and polarization curve analysis was performed at a constant potential of 1.6 V.

[0104] Assemble different porous diffusion layers into an effective area of ​​5*5cm 2 The PEM electrolyzer was used for polarization curve test, and the test current density range was from 0 to 2.0 A / cm2 , every 0.1A / cm 2 Record a voltage value. The test results are shown in Table 1:

[0105] Table 1

[0106] Porosity (%) <![CDATA[Contact resistance (mΩ·cm 2 )]]> <![CDATA[Corrosion current density (μA / cm 2 ).]]> <![CDATA[Electrolytic cell voltage (V) @ 1.6 A / cm 2 > Example 1 71 2.65 1.1 1.78 Example 2 68 3.61 1.1 1.82 Example 3 69 3.8 1.3 1.85 Example 4 66 3.83 2.7 1.95 Example 5 58 4.32 2.1 1.91 Example 6 57 4.53 1.8 1.95 Example 7 56 6.10 3.2 1.86 Example 8 51 4.11 2.5 1.88 Example 9 58 3.20 2.6 1.91 Comparative Example 1 48 4.68 2.9 1.93 Comparative Example 2 61 3.94 3.3 2.05 Comparative Example 3 59 13.67 17.9 2.25

[0107] As can be seen from Table 1, from Examples 1-3, the porosity of the porous transmission layer prepared by the method of the present invention can reach more than 68%, and the contact resistance can reach 3.8 mΩ·cm 2 Below, the corrosion current density can reach 1.3μA / cm 2 Below, performance tests in a PEM electrolyzer show that at 1.6A / cm 2 The voltage can reach below 1.85V at a current density of .

[0108] By comparing Example 1 with Examples 4-5, it can be seen that in the preparation process of the porous transmission layer of the present invention, the bias voltage of the non-precious metal coating and the precious metal coating will affect its performance. When the bias voltage of the non-precious metal coating and the precious metal coating is controlled at 100~300V, the performance of the porous transmission layer obtained is better. If the bias voltage is too high, the coating roughness is large and the corrosion resistance is poor; if the bias voltage is too low, the kinetic energy of the coated particles in the electric field is reduced, the deposition energy on the porous diffusion layer is reduced, the coating bonding strength is reduced, and the service life of the coating is reduced.

[0109] By comparing Example 1 with Examples 6-7, it can be seen that in the preparation process of the porous transport layer of the present invention, the temperature of the non-precious metal coating and the precious metal coating will affect its performance. When the temperature of the non-precious metal coating and the precious metal coating is controlled at 100-400°C, the performance of the porous transport layer is better. If the temperature is too high, the grains of the film layer grow abnormally, and stress concentration is likely to occur, resulting in the shedding of the coating; if the temperature is too low, the diffusion of the coating atoms is restricted, the coating structure is sparse, the coating has many defects, and the corrosion resistance is poor.

[0110] By comparing Example 1 with Examples 8-9, it can be seen that in the preparation process of the porous transmission layer described in the present invention, the air pressure of the non-precious metal coating and the precious metal coating will affect its performance. When the air pressure of the non-precious metal coating and the precious metal coating is controlled at 1~3Pa, the performance of the porous transmission layer obtained is better. If the air pressure is too high, the number of collisions of the coating particles in a vacuum increases, the mean free path of the particles decreases, the deposition energy is insufficient, and the coating bonding force is poor; if the air pressure is too low, the diffraction of the deposited particles is poor and the film uniformity is poor.

[0111] The contact resistance comparison diagram of the porous transport layer prepared in Examples 1-3 and Comparative Example 1 is shown in FIG. Figure 6 As shown, the performance test comparison of the PEM electrolyzer with porous transport layer prepared in Example 1 and Comparative Example 1 is shown in Figure 7As shown, by comparing Examples 1-3 with Comparative Example 1, the present invention adopts a vacuum coating (ion plating) process, the ions have good diffraction properties, and can be well deposited into the internal space of the porous transport layer, and due to the bombardment of high-energy ions, the coating has a large bonding force. The porosity of the porous transport layer is 2000 Å, and the conductive properties meet the current technical requirements, which is better than the existing technical products. The contact resistance performance is close to or even better than that of the traditional electroplated titanium felt. The electrolysis performance of the vacuum-coated titanium felt is more consistent than that of the commercial PEM electrolysis titanium felt.

[0112] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing a porous transport layer, It is characterized in that The preparation method comprises the following steps: (1) Glow cleaning of the substrate; (2) vacuum coating the glow-cleaned substrate, and obtaining the porous transmission layer after cooling; The vacuum coating process includes coating a non-precious metal coating on a substrate and then coating a precious metal on the non-precious metal coating.

2. The preparation method according to claim 1, It is characterized in that The substrate in step (1) includes any one of titanium mesh, titanium felt, titanium porous plate, metal mesh or composite porous conductive material, or a combination of at least two thereof.

3. The preparation method according to claim 1, It is characterized in that The step (1) is performed before the glow cleaning. The pretreatment includes degreasing-water washing-acid washing-water washing-vacuum drying; The mass concentration of the degreasing agent used in the degreasing is 0.1~1%; The degreasing time is 2 to 10 minutes; The pickling solution for pickling includes any one of oxalic acid, nitric acid or hydrofluoric acid or a combination of at least two thereof; The pickling time is 5 to 20 minutes; The temperature of the vacuum drying is 60-150°C; The vacuum degree of the vacuum drying is 1-100 Pa; The vacuum drying time is 20 to 40 minutes; The washing time is independently 1 to 3 minutes.

4. The preparation method according to claim 1, It is characterized in that The glow cleaning in step (1) includes cleaning the substrate in an inert atmosphere by means of negative glow discharge and an ion source; The bias voltage of the glow cleaning is 500-1000V; The pressure of the inert atmosphere is 0.1~100Pa; The ion source comprises any one of an anode layer ion source, a Hall ion source, a Kaufman ion source or a plasma source, or a combination of at least two thereof; The ion beam energy of the ion source is 100-500 eV; The cleaning time of the ion source is 5 to 30 minutes.

5. The preparation method according to claim 1, It is characterized in that The vacuum coating treatment device in step (2) includes a single vacuum coating furnace and / or a continuous vacuum coating furnace; The vacuum coating treatment method includes any one of vacuum evaporation, multi-arc ion plating, PECVD or magnetron sputtering, or a combination of at least two of them.

6. The preparation method according to claim 1, It is characterized in that The cooling time in step (2) is 3 to 20 minutes; The cooling atmosphere includes nitrogen and / or argon.

7. The preparation method according to claim 1, It is characterized in that The non-precious metal target material includes any one of Ti, Cr, W or Nb or a combination of at least two thereof; The coating method of the non-precious metal coating includes multi-arc ion plating and / or PECVD; The coating bias voltage of the non-precious metal coating is 50-500V; The air pressure of the non-precious metal coating is 0.1~10Pa; The coating gas for coating the non-precious metal coating includes any one of argon, nitrogen or methane, or a combination of at least two of them; The coating temperature of the non-precious metal coating is 60-600°C; The coating time of the non-precious metal coating is 5 to 20 minutes.

8. The preparation method according to claim 1, It is characterized in that The target material of the noble metal includes any one of Au, Pt, Ta or Ir or a combination of at least two thereof; The noble metal coating method includes multi-arc ion plating; The noble metal coating bias voltage is 50~500V; The gas pressure of the noble metal coating is 0.1~10Pa; The temperature of the precious metal coating is 60-600°C; The precious metal coating time is 1 to 5 minutes.

9. A porous transmission layer, It is characterized in that The porous transmission layer is prepared by the method according to any one of claims 1 to 8, and the porous transmission layer comprises a substrate and a non-precious metal film layer and a precious metal film layer sequentially stacked on at least one side of the substrate; The thickness of the non-precious metal film layer is 100-500 nm; The material of the non-precious metal film layer includes any one or a combination of at least two of Ti, Cr, Nb, W, and their nitrides, carbides or carbonitrides; The thickness of the noble metal film layer is 20-100 nm; The material of the noble metal film layer includes any one of Au, Pt, Ta or Ir, or a combination of at least two of them.

10. A PEM electrolyser, It is characterized in that The PEM electrolyzer comprises the porous transport layer of claim 9.

Citation Information

Patent Citations

  • Method for preparing protective coating on surface of bipolar plate of fuel cell

    CN108914060A

  • Porous transmission layer and PEM electrolytic bath

    CN116288457A

  • Composite coating, bipolar plate and porous diffusion layer

    CN116516382A

  • High-conductivity corrosion-resistant gas diffusion layer and preparation method thereof

    CN116837405A

  • Porous transport layer for use in a polymer electrolyte membrane electrolytic cell, electrolytic cell comprising said porous transport layer, method for obtaining said porous transport layer and

    CN118525112A